All-synthetic grinding fluid
A kind of grinding fluid, fully synthetic technology, applied in the field of grinding fluid, can solve the problems of short anti-rust cycle, affecting the appearance of workpiece, surface finish, poor precision, etc., to achieve no harm to the body, no pollution to the environment, and anti-rust cycle long effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] 1. Put 200kg of water, 100kg of diethylene glycol, 20kg of JFC and 100kg of polyether into the reaction kettle, heat to 72 degrees and stir for 60 minutes until they are completely dissolved.
[0013] 2. Put 20kg of borax and 2kg of organic molybdenum into 296kg of water, fully dissolve and add them into the above reaction kettle, and stir evenly.
[0014] 3. Adjust 20kg of dimer acid, 30kg of octanoic acid and 200kg of triethanolamine at 70°C and mix them evenly. After they appear bright reddish brown, add them into the above reaction kettle and stir evenly.
[0015] 4. Add 1.25 kg of silicone defoamer and 12.5 kg of tributyl phosphate, stir evenly, and obtain a light yellow fully synthetic grinding fluid product.
Embodiment 2
[0017] 1. Put 260kg of water, 100kg of diethylene glycol and 100kg of polyether into the reaction kettle, heat to 72 degrees and stir for 60 minutes until they are completely dissolved.
[0018] 2. Put 20kg of borax and 2kg of organic molybdenum into 296kg of water, fully dissolve and add them into the above reaction kettle, and stir evenly.
[0019] 3. Mix 20kg of dimer acid and 200kg of diethanolamine at 70 degrees and add them into the above reaction kettle after they appear bright reddish brown, and stir evenly.
[0020] 4. Add 1.25 kg of silicone defoamer and 12.5 kg of tributyl phosphate, stir evenly, and obtain a light yellow fully synthetic grinding fluid product.
Embodiment 3
[0022] 1. Put 260kg of water, 100kg of diethylene glycol and 100kg of polyether into the reaction kettle, heat to 72 degrees and stir for 60 minutes until they are completely dissolved.
[0023] 2. Put 20kg of borax into 296kg of water, fully dissolve and add it into the above reaction kettle, and stir evenly.
[0024] 3. Adjust 20kg of dimer acid, 40kg of caprylic acid, 50kg of diethanolamine and 150kg of triethanolamine at 70°C and mix them evenly. After they appear bright reddish brown, add them to the above reaction kettle and stir evenly.
[0025] 4. Add 1.25 kg of silicone defoamer and 12.5 kg of tributyl phosphate, stir evenly, and obtain a light yellow fully synthetic grinding fluid product.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com