Low-temperature activating and bleaching method by using water-soluble metalloporphyrin
A metalloporphyrin, low-temperature activation technology, applied in the field of low-temperature activation and bleaching, can solve the problems of rough hand feeling, difficult penetration and low production efficiency of fabrics, and achieve the effects of reducing the pH of the working solution and shortening the stacking time.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] (1) Preparation of bleaching liquid
[0035] Prepare the bleach in a 1000ml beaker, its components are, H 2 o 2 (30%) 30g / L, cobalt porphyrin tetrasulfonate 9 μmol / L, adjust the working solution to 7 with NaOH, penetrant 2g / L, stabilizer 0.2g / L.
[0036] (2) Padding process
[0037] Keep the liquid-carrying rate of 90%-100%, two dipping and two rolling.
[0038] (3) Steaming process
[0039] After padding the bleaching solution, put the fabric into a sealed bag and seal it tightly, and steam it in a blast oven at 80°C for 1 hour.
[0040] (4) Washing and drying
[0041] Wash in hot water, wash in cold water and tumble dry in forced air oven.
Embodiment 2
[0043] (1) Preparation of bleaching liquid
[0044] Prepare the bleach in a 1000ml beaker, its components are, H 2 o 2 (30%) 30g / L, cobalt porphyrin tetrasulfonate 6 μmol / L, adjust the working solution to 9.5 with NaOH, penetrant 2g / L, stabilizer 0.2g / L.
[0045] (2) Padding process
[0046] Keep the liquid-carrying rate of 90%-100%, two dipping and two rolling.
[0047] (3) Steaming process
[0048] After padding the bleaching solution, put the fabric into a sealed bag and seal it tightly, and steam it in a blast oven at 80°C for 1 hour.
[0049] (4) Washing and drying
[0050] Wash in hot water, wash in cold water and tumble dry in forced air oven.
Embodiment 3
[0052] (1) Preparation of bleaching liquid
[0053] Prepare the bleach in a 1000ml beaker, its components are, H 2 o 2 (30%) 30g / L, tetrasulfonate cobalt porphyrin 3 μmol / L. Regulate working solution with NaOH to 9.5, penetrant 2g / L, stabilizer 0.2g / L.
[0054] (2) Padding process
[0055] Keep the liquid-carrying rate of 90%-100%, two dipping and two rolling.
[0056] (3) Steaming process
[0057] After padding the bleaching solution, put the fabric into a sealed bag and seal it tightly, and steam it in a blast oven at 80°C for 1 hour.
[0058] (4) Washing and drying
[0059] Wash in hot water, wash in cold water and tumble dry in forced air oven.