[0028] A kind of sodium hypochlorite printing technique, comprises the following steps:
[0029] 1. Add 400ml of 120g / l sodium hypochlorite, 700g of sodium alginate, 20g of soda ash, 50g of sodium hexametaphosphate and 5ml of formaldehyde with a concentration of 40% in 7000g of water at 65°C, add water and stir to synthesize 10kg of paste, and then use glacial acetic acid to dissolve the paste The PH value of the material is adjusted to 6-8, and it is made into printing paste.
[0030] 2. Through the machine continuous printing or manual intermittent printing process, engrave the patterned screen or roller, print the slurry on the piece or sheet fabric, and dry it at 65 degrees.
[0031] 3. After the above fabrics are made into clothes, wash them with water, sand or suspended stones.
Embodiment 2
[0033] A kind of sodium hypochlorite printing technique, comprises the following steps:
[0034] 1. Add 400ml of 100g / l sodium hypochlorite, 600g of sodium alginate, 15g of soda ash, and 45g of sodium hexametaphosphate to 6500g of water at 60°C, add water and stir to form a 10kg paste, then use glacial acetic acid to adjust the pH value of the paste to 6-8 , made into printing paste.
[0035] 2. Through the machine continuous printing or manual intermittent printing process, engrave the patterned screen or roller, print the slurry on the piece or sheet fabric, and dry it at 50 degrees.
[0036] 3. After the above fabrics are made into clothes, wash them with water, sand or suspended stones.
Embodiment 3
[0038] A kind of sodium hypochlorite printing technique, comprises the following steps:
[0039] 1. Add 400ml of 140g / l sodium hypochlorite, 800g of sodium alginate, 25g of soda ash, 55g of sodium hexametaphosphate and 10ml of formaldehyde with a concentration of 40% in 7500g of 70°C water, add water and stir to form 10kg of paste, and then use glacial acetic acid to dissolve the paste The PH value of the material is adjusted to 6-8, and it is made into printing paste.
[0040] 2. Through the machine continuous printing or manual intermittent printing process, engrave the patterned screen or roller, print the slurry on the piece or sheet fabric, and dry it at 80 degrees.
[0041] 3. After the above fabrics are made into clothes, wash them with water, sand or suspended stones.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com