A technology of curing paint and ultraviolet light, which is applied to the device for coating liquid on the surface, coating, pretreatment surface, etc., which can solve the problems of paint film cracking, paint film peeling, economic loss, etc., and prevent paint film from bubbling , good surface effect, less environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Embodiment 1: The spraying construction technology that prevents the paint film of medium density board to be coated with from turning white
[0036] The object to be coated is a decorative material composed of medium density boards, and the object to be coated is carried out to prevent the construction method of the UV-cured paint film from foaming, comprising the following steps:
[0037] 1) Sanding the object to be coated: use sandpaper to sand the burr of the object, and sand it smooth;
[0038] 2) Coloring of the object to be coated: use ultraviolet light to color the high-adhesion primer (top primer), evenly roller coat, and UV curing machine to cure and dry completely;
[0039] 3) Sanding: use sandpaper to sand flat and smooth;
[0040] 4) Adjust the construction viscosity of the UV-curable spray transparent primer (surfacer) to 16 seconds with a special thinner for UV-curable activity, and spray a "ten" evenly, with a temperature of 40°C and a length of 10 mete...
Embodiment 2
[0049] Embodiment 2: the roller coating construction method that prevents solid wood to be coated with paint film foaming
[0050] The object to be coated is a decorative material composed of solid wood. A construction method for preventing blistering of an ultraviolet light-cured paint film on an object comprises the following steps:
[0051] 1) Sanding the object to be coated: use sandpaper to sand the burr of the object, and sand it smooth;
[0052] 2) Coloring of the object to be coated: use ultraviolet light to color the high-adhesion primer (top primer), apply it evenly with a roller, and UV cure and semi-dry;
[0053] 3) Ultraviolet light transparent primer; roller coating is applied with ultraviolet light curing roller coating transparent primer (surfacer), and the construction viscosity is adjusted to 18 seconds with a special thinner for ultraviolet light curing activity, and the temperature is 50 °C and the length is 10 meters. The infrared leveling machine levele...
Embodiment 3
[0062] Embodiment 3: The spraying construction technology that prevents the medium density board to be coated with paint film from turning white
[0063] The object to be coated is a decorative material composed of medium density boards, and the object to be coated is carried out to prevent the construction method of the UV-cured paint film from foaming, comprising the following steps:
[0064] 1) Sanding the object to be coated: use sandpaper to sand the burr of the object, and sand it smooth;
[0065] 2) Coloring of the object to be coated: use ultraviolet light to color the high-adhesion primer (top primer), evenly roller coat, and UV curing machine to cure and semi-dry;
[0066] 3) Adjust the construction viscosity of the UV-curable spray transparent primer (surfacer) to 14 seconds with a special thinner for UV-curable activity, and spray a "ten" evenly, with a temperature of 45°C and a 10-meter-long UV-IR flow Flat for 4 minutes, the UV curing machine is completely dry; ...