Embodiment 1
[0034] Base layer material: 100g o-phthalic unsaturated polyester resin, 100g isophthalic unsaturated polyester resin, 1g benzoyl peroxide, 2g cobalt naphthenate, 200g quartz sand, 10g acetone solvent; mix and stir evenly.
[0035] Surface layer material: 100g o-phthalic unsaturated polyester resin, 100g isophthalic unsaturated polyester resin, 2g benzoyl peroxide, 1g cobalt naphthenate, 200g aluminum hydroxide powder, 10g acetone solvent; mix and stir evenly .
[0036] Craftsmanship:
[0037] The product mold is repaired, cleaned, waxed and polished, and then the surface layer material liquid is sprayed around the inside of the mold, and then the matrix layer material liquid is poured into the mold. After curing, it is stripped, trimmed, cut, and finally packaged to obtain the finished product.
[0038] This product does not pollute the environment and is safe to use. The production process of this product is simple, the color can be adjusted, and it can be poured and form...
Embodiment 2
[0040] Base layer material: 100g o-phthalic unsaturated polyester resin, 100g isophthalic unsaturated polyester resin, 4g benzoyl peroxide, 1g cobalt naphthenate, 400g quartz sand, 15g acetone solvent; mix and stir evenly.
[0041] Surface layer material: 100g o-phthalic unsaturated polyester resin, 100g isophthalic unsaturated polyester resin, 1g benzoyl peroxide, 3g cobalt naphthenate, 300g aluminum hydroxide powder, 12g acetone solvent; mix and stir evenly .
[0042] Manufacturing process is the same as embodiment 1.
[0043] In the present invention, the ratio of resin to inorganic filler is controlled at about 1:1-2, and at the same time, the method of using o-phthalic and iso-phthalic resins in combination to make up for each other's defects, and the curing time and performance of the same type of resin are different Not too large, so that the properties of the prepared product matrix and the surface layer are the same, and also maintain strong toughness and hardness, w...