Embodiment 1
[0023] A concrete pumping agent provided in this embodiment is mainly composed of β-naphthalenesulfonic acid formaldehyde condensate, calcium lignosulfonate, air-entraining agent, starch, and water.
[0024] It can be used, but not limited to, the following methods of use:
[0025] Add β-naphthalenesulfonic acid formaldehyde condensate, calcium lignosulfonate, air-entraining agent, starch, and water to the cement concrete in a predetermined proportion to make the reaction occur, and then add starch to the reactant in a predetermined proportion, Continue to stir for condensation reaction.
[0026] It can be seen from the above that since the concrete pumping agent of this embodiment contains β-naphthalenesulfonic acid formaldehyde condensate and starch, the β-naphthalenesulfonic acid formaldehyde condensate and starch can be polymerized when they are mixed into cement concrete Reaction can significantly improve the mechanical properties, working performance and durability of c...
Embodiment 2
[0029] The weight ratio of the pumping agent of the present embodiment is as follows: 20% of β-naphthalenesulfonic acid formaldehyde condensate, 6% of calcium lignosulfonate, 0.1% of air-entraining agent (SJ-2 air-entraining agent), 10% of starch, Water 50%.
[0030] Its use method is as follows: Add 20% of β-naphthalenesulfonic acid formaldehyde condensate, 6% of calcium lignosulfonate, 0.1% of air-entraining agent (SJ-2), and 50%-65% of water in proportion to make it react; Then, 10% starch by weight is added in proportion to the reactants, and the stirring is continued to carry out the condensation reaction.
[0031] Wherein the denominator of the above weight ratio is the total weight of the β-naphthalenesulfonic acid formaldehyde condensate, calcium lignosulfonate, air-entraining agent and starch.
Embodiment 3
[0033] The weight ratio of the pumping agent in this embodiment is as follows: 30% of β-naphthalenesulfonic acid formaldehyde condensate, 12% of calcium lignosulfonate, 0.2% of air-entraining agent, 25% of starch, and 65% of water.
[0034] Its use method is as follows: Add 30% of β-naphthalenesulfonic acid formaldehyde condensate, 12% of calcium lignosulfonate, 0.2% and 65% of air-entraining agent (SJ-2) in proportion to make it react; Add starch with a weight ratio of 25% into the mixture in proportion, and continue stirring to carry out condensation reaction.
[0035] Wherein the denominator of the above weight ratio is the total weight of the β-naphthalenesulfonic acid formaldehyde condensate, calcium lignosulfonate, air-entraining agent and starch.