Method for performing crease-resistant finishing on cotton textile fabrics or garments
A cotton textile, anti-wrinkle finishing technology, applied in textile and papermaking, textile material processing, spray/jet textile material processing and other directions, can solve the problems of needing ironing, poor elasticity, easy to wrinkle and so on
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] Put the all-cotton textile fabric or garment into the rotating cage of the spraying machine, and spray the anti-wrinkle lotion evenly on the all-cotton textile fabric or garment through the 0.45MP high-pressure nozzle of the spraying machine; the all-cotton textile fabric or The weight ratio of ready-made clothes and anti-wrinkle lotion is 1:1.05; start the high-pressure spraying machine, cotton textile fabrics or ready-made clothes are in the high-pressure spraying machine, turn the cage forward and backward regularly, and spray the lotion in 15 minutes Complete, after the spraying is completed, the cage continues to rotate for 10 minutes; the composition of the anti-wrinkle lotion includes: water, glyoxal resin, 30%-50% magnesium chloride solution by weight, lubricating softener, high polyethylene type Lubricating agent, amino silicone oil softener, penetrating agent 230, brightener; The compound method of described anti-wrinkle liquid medicine: add 160 gram glyoxal re...
Embodiment 2
[0036] Put the all-cotton textile fabric or garment into the rotating cage of the spraying machine, and spray the anti-wrinkle lotion evenly on the all-cotton textile fabric or garment through the 0.6MP high-pressure nozzle of the spraying machine; the all-cotton textile fabric or The weight ratio of ready-made clothes and anti-wrinkle lotion is 1:1.05; start the high-pressure spraying machine, cotton textile fabrics or ready-made clothes are in the high-pressure spraying machine, turn the cage forward and backward regularly, and spray the lotion in 20 minutes Complete, after the spraying is completed, the cage continues to rotate for 10 minutes; the composition of the anti-wrinkle lotion includes: water, glyoxal resin, 30%-50% magnesium chloride solution by weight, lubricating softener, high polyethylene type Lubricating agent, amino silicone oil softener, penetrating agent 230, brightener; The preparation method of described anti-wrinkle liquid medicine: add 170 gram glyoxal ...
Embodiment 3
[0043] Put the all-cotton textile fabric or garment into the rotating cage of the spraying machine, and spray the anti-wrinkle lotion evenly on the all-cotton textile fabric or garment through the 0.5MP high-pressure nozzle of the spraying machine; the all-cotton textile fabric or The weight ratio of ready-made clothes and anti-wrinkle lotion is 1:1.05; start the high-pressure spraying machine, cotton textile fabrics or ready-made clothes are in the high-pressure spraying machine, turn the cage forward and backward regularly, and spray the lotion in 18 minutes Complete, after the spraying is completed, the cage continues to rotate for 10 minutes; the composition of the anti-wrinkle lotion includes: water, glyoxal resin, 30%-50% magnesium chloride solution by weight, lubricating softener, high polyethylene type Lubricant, amino silicone oil softener, penetrating agent 230, whitening agent; The preparation method of described anti-wrinkle syrup: 165 gram glyoxal resins are added ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com