A method of utilizing potassium feldspar to manufacture potassium sulfate fertilizer and co-produce special cement
A technology of special cement and potassium feldspar, which is applied in the fields of potash fertilizer, cement production, chemical instruments and methods, etc., can solve the problems of low output ratio of potassium sulfate, unhandy tailings, and environmental pollution, and achieve short industrial chain and low investment Small size and low energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Embodiment one: utilize potassium rock to manufacture potassium sulfate fertilizer co-production special cement, it is to collect potassium sulfate in kiln tail dust collection cover earlier, then the slag that kiln head is discharged is produced special cement such as radiation-resistant cement, white cement, its production method Including the following steps:
[0022] Prepare materials: first prepare the following materials in parts by weight, potassium rock 40, limestone 40, barite 18, fluorite 2, total 100;
[0023] Crushing: firstly crush potassium rock, limestone, barite and fluorite to less than 20mm and pre-homogenize;
[0024] Batching grinding and homogenization: the materials obtained in step 2 are mixed according to the ratio of step 1, and then put into the grinding mill, and the raw materials pass through a 180-200 mesh sieve and put into storage for homogenization;
[0025] Calcination: Homogenized qualified raw meal (TCaCO 3 No more than ±0.2%...
Embodiment 2
[0030] Embodiment two: utilize potassium rock to manufacture potash fertilizer co-production special cement, as anti-radiation cement or white cement, its production method comprises the steps: Prepare materials: first prepare the following materials by weight percentage, potassium rock 38, limestone 41, barite 20, fluorite 1, the total amount is 100;
[0031] Crushing: firstly crush potassium rock, limestone, barite and fluorite to less than 20mm and pre-homogenize;
[0032] Batching grinding and homogenization: the materials obtained in step 2 are mixed according to the ratio of step 1, and then put into the grinding mill, and the raw materials pass through a 180-200 mesh sieve and put into storage for homogenization;
[0033] Calcination: Homogenized qualified raw meal (TCaCO 3 Not exceeding ±0.2%) into the kiln for calcination, and the firing temperature is controlled at 1350°C to 1400°C;
[0034] The production of potash fertilizer:
[0035] A. Potassium sulfa...