Preparation process for preparing kaolin with high brightness by using coal gangues
A preparation process, kaolin technology, applied in the direction of aluminum silicate, silicate, etc., can solve the problems of not achieving the ideal effect, affecting the practical application, environmental pollution, etc., and achieve the effect of low cost, small investment and good effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] First of all, the raw material coal gangue ore has been analyzed for components and XRD for many times, and the results are as follows:
[0039]
[0040] According to the above phase analysis, the following preparation process of high whiteness kaolin is determined:
[0041] A preparation process for preparing high-whiteness kaolin from coal gangue, comprising the following steps:
[0042] A, crushing, crushing raw ore coal gangue, the crushed particle size is 0.1mm ~ 2mm;
[0043] B, jigging, using an asymmetric sine wave jig to carry out jigging operations on the crushed coal gangue in step A, to separate coarse pyrite, and the iron removal rate is 63%; Most of the pyrite has been removed after two re-elections.
[0044] C, grinding, and then grinding the remaining ore particles in step B to 0.047mm~0.1mm;
[0045] D, particle selection, the ore particles in the step C are pumped into the spiral chute for re-election, and the fine-grained pyrite is separated;
...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle size | aaaaa | aaaaa |
| whiteness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information