A kind of formaldehyde color test paper and its preparation method and application
A formaldehyde and test paper technology, applied in the field of formaldehyde color development test paper and its preparation, can solve the problems of reduced formaldehyde removal rate, low concentration, irreversibility, etc., and achieve the effect of real-time correlation and formaldehyde sensitivity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] A formaldehyde color test paper, specifically prepared by the method comprising the following steps:
[0025] (1) According to the ratio of ammonium acetate: glacial acetic acid: acetylacetone of 25g: 3mL: 0.5 mL, mix 25g of ammonium acetate, 3mL of glacial acetic acid and 0.5mL of acetylacetone to dissolve, then add purified water and dilute to 100ml. Obtain the mixed solution 1 that the volume percent concentration of acetylacetone is 0.5%;
[0026] (2) Add 100g of water-soluble polyacrylic acid resin into 100ml of mixed solution 1 obtained in step (1), stir and mix evenly to obtain mixed solution 2;
[0027] The amount of water-soluble polyacrylic resin added is calculated according to the ratio of water-soluble polyacrylic resin: the mixed solution 1 obtained in step (1) is 1g:1ml;
[0028] (3) After soaking the kapok paper in the mixed solution 2 obtained in step (2) for 2 hours, air-dry naturally in the air to obtain the formaldehyde color test paper.
[0029] U...
Embodiment 2
[0036] A formaldehyde color test paper, specifically prepared by the method comprising the following steps:
[0037] (1) According to the ratio of ammonium acetate: glacial acetic acid: acetylacetone of 25g:3mL:1mL, mix 25g of ammonium acetate, 3mL of glacial acetic acid and 1mL of acetylacetone to dissolve, then add purified water and dilute to 100ml to obtain acetylacetone The volume percent concentration of acetone is a mixed solution 1 of 1%;
[0038] (2) Add 150g of water-soluble polyacrylic acid resin into 100ml of mixed solution 1 obtained in step (1), stir and mix evenly to obtain mixed solution 2;
[0039] The amount of water-soluble polyacrylic resin added is calculated according to the ratio of water-soluble polyacrylic resin: the mixed solution 1 obtained in step (1) is 1.5g: 1ml;
[0040] (3) After soaking the kapok paper in the mixed solution 2 obtained in step (2) for 2 hours, air-dry naturally in the air to obtain the formaldehyde color test paper.
[0041] U...
Embodiment 3
[0048] A formaldehyde color test paper, specifically prepared by the method comprising the following steps:
[0049] (1) According to the ratio of ammonium acetate: glacial acetic acid: acetylacetone of 25g: 3mL: 1.5mL, mix 25g of ammonium acetate, 3mL of glacial acetic acid and 1.5mL of acetylacetone to dissolve, then add purified water and dilute to 100ml. Obtaining the volume percent concentration of acetylacetone is a mixed solution 1 of 1.5%;
[0050](2) Add 200g of water-soluble polyacrylic acid resin into 100ml of mixed solution 1 obtained in step (1), stir and mix evenly to obtain mixed solution 2;
[0051] The amount of water-soluble polyacrylic acid resin added is calculated according to the ratio of water-soluble polyacrylic resin: mixed solution 1 obtained in step (1) is 2g:1ml;
[0052] (3) After soaking the kapok paper in the mixed solution 2 obtained in step (2) for 2 hours, air-dry naturally in the air to obtain the formaldehyde color test paper.
[0053] Use...
PUM

Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations