A processing method and sheepskin technology, applied in chemical treatment before tanning, small raw hide/large raw hide/leather/fur treatment, small raw hide/large raw hide/leather hide/fur chemical treatment, etc. Clothes and other problems, to achieve the effect of simple steps, strong durability and easy operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] A method for processing sheepskin, said method comprising the following steps:
[0026] Step 1, at a temperature of 5°C, brush the peeled sheepskin with salt water to ensure that the sheepskin is in a state of salt water infiltration, and hang the sheepskin in a cool place for 8 to 10 days after 7 days;
[0027] Step 2, at a temperature of 2°C, smear yogurt on the surface of the sheepskin, then fold the skin and place it, and reapply yogurt every two days for 12 days;
[0028] Step 3, hanging the sheepskin in a cool and ventilated place at a temperature of -5-10°C for 8-10 days; scraping off impurities on the surface of the sheepskin, washing and drying; kneading to obtain the treated sheepskin.
[0029] The prepared sheepskin is made into a sheepskin cushion, and the durability of the period is observed after one year of normal use; after one year of normal use, the appearance of the sheepskin is good, and the wool shedding is less than 10%.
[0030] A sheepskin odor ...
Embodiment 2
[0032] On the one hand, the embodiment of the present invention provides a kind of sheepskin processing method, described method comprises the following steps:
[0033] Step 1, at the temperature of -4°C, brush the peeled sheepskin with salt water to ensure that the sheepskin is in a state of salt water infiltration, and hang the sheepskin in a cool place for 8 to 10 days after 7 days;
[0034] Step 2, at a temperature of 2°C, smear yogurt on the surface of the sheepskin, then fold the skin and place it, and reapply yogurt every two days for 12 days;
[0035] Step 3, hanging the sheepskin in a cool and ventilated place at a temperature of -5-10°C for 8-10 days; scraping off impurities on the surface of the sheepskin, washing and drying; kneading to obtain the treated sheepskin.
[0036] The prepared sheepskin is made into a sheepskin cushion, and the durability of the period is observed after one year of normal use; after one year of normal use, the appearance of the sheepskin...
Embodiment 3
[0039] On the one hand, the embodiment of the present invention provides a kind of sheepskin processing method, described method comprises the following steps:
[0040] Step 1, at a temperature of 10°C, brush the peeled sheepskin with salt water to ensure that the sheepskin is in a state of salt water infiltration, and hang the sheepskin in a cool place for 8 to 10 days after 7 days;
[0041] Step 2, at a temperature of 2°C, smear yogurt on the surface of the sheepskin, then fold the skin and place it, and reapply yogurt every two days for 12 days;
[0042] Step 3, hanging the sheepskin in a cool and ventilated place at a temperature of -5-10°C for 8-10 days; scraping off impurities on the surface of the sheepskin, washing and drying; kneading to obtain the treated sheepskin.
[0043] The prepared sheepskin is made into a sheepskin cushion, and the durability of the period is observed after one year of normal use; after one year of normal use, the appearance of the sheepskin i...