Embodiment 1
[0165] A) Preparation of gypsum block and gypsum board
[0166] Add 820kg of water into the mixing tank, then add 12kg of water reducer (SM), 1.5kg of sodium lauryl sulfate, then add 350kg of hemihydrate gypsum, 220kg of ordinary Portland cement (type 425), 280kg of fly ash and Polybutadiene rubber (PBR) powder (200um average particle size) 6Kg mixed powder. High-speed stirring, stirring speed 400-800rpm. Stirring time 20-30s. The measured wet bulk density of the slurry material (or concrete) is 1.63 tons / cubic meter. Then respectively in the block mold that inner surface has been coated with potassium soap mold release agent and inner surface has been coated with potassium soap mold release agent and has packed into three-dimensional steel framework (thickness t=12cm, length l=3.0 meters, Width w=0.6m, where the width of the steel skeleton is in the vertical direction, the length and thickness of the steel skeleton are in the horizontal direction, and two layers of steel w...
Embodiment 2
[0172] A) Preparation of gypsum blocks and gypsum boards: Example 1 was repeated, except that the amount of water added was 860 kg and 100 kg of lignocellulose was further added before stirring. The wet bulk density of the slurry (or concrete) is 1.58 tons / m3.
[0173] B) Performance index of gypsum block and gypsum board
[0174] The index of the finished block is: dry bulk density 801kg / m 3 , compressive strength 16.3Mpa, thermal conductivity 0.09w / ㎡·℃, frost resistance cycle ≥ 30, fire resistance class A, softening coefficient 0.81, water resistance ≥ 10 years, can be soaked in water for several years without softening.
[0175] According to the upper and lower positions of the block or plate when it is poured, sample 8cm from the surface and bottom of the hardened block or plate. 3 Cube, weighing, measured: the density of the surface sample of the block (i.e. the surface layer density) is 798kg / m 3 , the density of the bottom sample of the block (that is, the bottom lay...
Embodiment 3
[0177] Repeat embodiment 1, just the addition of polybutadiene rubber (PBR) powder is 10Kg, and SDS consumption is 0.1Kg.
PUM
| Property | Measurement | Unit |
|---|---|---|
| diameter | aaaaa | aaaaa |
| length | aaaaa | aaaaa |
| width | aaaaa | aaaaa |