Anti-yellowing priming paint
A technology of anti-yellowing and primer, which is applied in the direction of coating, etc., can solve the problems of poor anti-yellowing ability of the primer, and achieve the effects of broad market prospects, quality improvement, and strong anti-yellowing ability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0043] The preparation method of primer described in above-mentioned technical scheme is preferably:
[0044] The acrylic resin, pentachlorobiphenyl, auxiliary agent and solvent are mixed to obtain the first mixture; the linseed oil and titanium dioxide are mixed for the second time to obtain the second mixture; the second mixture, filler and bentonite are subjected to the second mixture 3. Mix to get the primer.
[0045] The above-mentioned three times of mixing are all realized by stirring, and the speed of stirring during the three times of mixing is preferably 800 rpm to 1000 rpm, and the time of each mixing and stirring is 30 minutes.
Embodiment 1
[0048] Described anti-yellowing primer, wherein, is made up of following components in parts by weight:
[0049] 45 parts of acrylic resin;
[0050] 15 parts of pentachlorobiphenyl;
[0051] 10 parts of linseed oil;
[0052] 5 parts of titanium dioxide;
[0053] 20 parts of filler;
[0054] 2 parts of bentonite;
[0055] 1 part of auxiliary agent;
[0056] 10 parts of solvent.
[0057] The preparation method of the primer described in the above technical scheme is: mix acrylic resin, pentachlorobiphenyl, auxiliary agent and solvent, stir according to 800 rpm, and the stirring time is 30 minutes, to obtain the first mixture; The oil and titanium dioxide were mixed for the second time, stirred at 800 rpm, and the stirring time was 30 minutes to obtain the second mixture; the second mixture, filler and bentonite were mixed for the third time, stirred at 800 rpm, and the stirring time was For 30 minutes, get the primer.
[0058] The primer obtained in Example 1 of the pres...
Embodiment 2
[0060] Described anti-yellowing primer, wherein, is made up of following components in parts by weight:
[0061] 40 parts of acrylic resin;
[0062] 15 parts of pentachlorobiphenyl;
[0063] 10 parts of linseed oil;
[0064] Titanium dioxide 8 parts
[0065] 20 parts of filler;
[0066] 1 part bentonite;
[0067] 5 parts of auxiliary agent;
[0068] 15 parts of solvent.
[0069] The preparation method of the primer described in the above technical scheme is: mix acrylic resin, pentachlorobiphenyl, auxiliary agent and solvent, stir according to 1000 rpm, and the stirring time is 30 minutes, to obtain the first mixture; The oil and titanium dioxide are mixed for the second time, stirred at 1000 rpm, and the stirring time is 30 minutes to obtain the second mixture; the second mixture, filler and bentonite are mixed for the third time, stirred at 1000 rpm, and the stirring time is For 30 minutes, get the primer.
[0070] The primer obtained in Example 2 of the present inve...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com