A new type of textile technology, applied in the field of apparel textiles, can solve the problems of down jacket running down, low weight gain anti-drilling down, cold resistance, moisture permeability, washing resistance, down drilling and other problems, and achieves good down-proof, low cost, The effect of improving production efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0061] A novel cashmere-proof process for textiles is characterized in that it comprises the following steps:
[0062] (1) Fabric selection: plain fabric woven with nylon FDY fully stretched yarn, yarn count 40D*40D, density 290T;
[0063] (2) Perform water-repellent finishing on the fabric, and the water-staining level is ≥3;
[0064] (3) Calender the fabric after water-repellent finishing with a calender, with a pressure of 10MPa, a temperature of 110°C, and a vehicle speed of 35m / min;
[0065](4) Coating glue preparation, raw material weight ratio:
[0066] 100 parts of environmentally friendly polyurethane resin coating glue;
[0067] 0.4 parts of defoamer;
[0068] 1.8 parts of associative polyurethane rheology additive;
[0069] 8 parts of hand feeling agent;
[0070] 25 parts of hydroxyl-terminated polydimethylsiloxane emulsion;
[0071] 1.3 parts of isocyanate crosslinking agent;
[0072] 1.6 parts of cross-linking accelerator;
[0073] 4 parts of silica mattin...
Embodiment 2
[0087] A novel cashmere-proof process for textiles is characterized in that it comprises the following steps:
[0088] (1) Fabric selection: plain fabric woven with nylon FDY fully stretched yarn, yarn count 20D*20D, density 370T;
[0089] (2) Perform water-repellent finishing on the fabric, and the water-staining level is ≥3;
[0090] (3) Calender the fabric after water-repellent finishing with a calender, with a pressure of 11MPa, a temperature of 110°C, and a vehicle speed of 40m / min;
[0091] (4) Coating glue preparation, raw material weight ratio:
[0092] 100 parts of environmentally friendly polyurethane resin coating glue;
[0093] 0.5 part of defoamer;
[0094] 2.0 parts of associative polyurethane rheology additive;
[0095] 9 parts of hand feeling agent;
[0096] 28 parts of hydroxyl-terminated polydimethylsiloxane emulsion;
[0097] 1.5 parts of isocyanate crosslinking agent;
[0098] 1.8 parts of cross-linking accelerator;
[0099] 5 parts of silica mattin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com