Rosewood treatment method
A treatment method, mahogany technology, applied in wood treatment, wood treatment details, impregnated wood, etc., can solve the problems of unqualified wood drying process, vulnerability to insects, and defects of drying tools, so as to improve wood utilization rate, Good drying quality and fast drying effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0040] A method for drying mahogany wood, comprising the following steps:
[0041] 1) Poaching: Dismember the mahogany wood into a plate shape, then completely immerse the mahogany board in water at 80 degrees Celsius and boil for 10 days; then conduct a cooling oil seepage: naturally cool the boiled mahogany to make it set once And finished with mahogany oil exudation;
[0042] 2), steaming: the mahogany wood in step 1) is sealed and steamed for 13 days in the steam of 70 degrees Celsius under 1.7 atmospheric pressure; the wood is separated by wooden supports of the same specification, so that the wood is evenly heated and baked. The dried wood is naturally cooled in the drying box, and the secondary cooling and oil seepage is carried out to make the secondary setting and the external oil leakage of mahogany is completed;
[0043]3) Second steaming: steam the mahogany wood in step 2) in steam at 60 degrees Celsius under 1.3 atmospheric pressure for 13 days; then three times ...
Embodiment 2
[0048] A method for drying mahogany wood, comprising the following steps:
[0049] 1) Poaching: Dismember the mahogany wood into a plate shape, then completely immerse the mahogany board in water at 70 degrees Celsius and boil for 8 days; then conduct a cooling oil seepage: naturally cool the boiled mahogany to make it shape once And finished with mahogany oil exudation;
[0050] 2), steaming: the mahogany wood in step 1) is sealed and steamed for 17 days in the steam of 65 degrees Celsius under 1.7 atmospheric pressure; the wood is separated by wooden supports of the same specification, so that the wood is evenly heated and baked. The dried wood is naturally cooled in the drying box; after secondary cooling, the oil is released;
[0051] 3) Second steaming: Steam the mahogany wood in step 2) in steam at 50 degrees Celsius under 1.4 atmospheres for 17 days; then three times of cooling: naturally cool the steamed mahogany;
[0052] 4), vacuum high-frequency drying: the mahoga...
Embodiment 3
[0056] A method for drying mahogany wood, comprising the following steps:
[0057] 1) Poaching: Dismember the mahogany wood into a plate shape, then completely immerse the mahogany board in water at 75 degrees Celsius and boil for 6 days; then conduct a cooling oil seepage: naturally cool the boiled mahogany to make it shape once And finished with mahogany oil exudation;
[0058] 2), steaming: the mahogany wood in step 1) is sealed and steamed for 16 days in the steam of 70 degrees Celsius under 1.6 atmospheric pressure; the wood is separated by wooden supports of the same specification, so that the wood is evenly heated and baked. The dried wood is naturally cooled in the drying box; after secondary cooling, the oil is released;
[0059] 3), secondary steaming: the mahogany wood of step 2) is sealed and steamed for 15 days under 1.4 atmospheric pressure in the steam of 50 degrees centigrade; then three times of cooling: the mahogany after steaming is carried out natural cool...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com