preparation example Construction
[0191] The present invention also provides a preparation method of the composition, comprising the steps of:
[0192] 1) providing the first mixed solution and the second mixed solution, wherein,
[0193] The first mixed solution contains: 3-30 parts by weight of pearlescent pigment, 20-25 parts by weight of glass beads and optionally 25-50 parts by weight of water;
[0194] The second mixed liquid contains: 10-40 parts by weight of emulsion;
[0195] 2) Mixing the first mixed liquid and the second mixed liquid under stirring condition to obtain the composition.
[0196] In another preferred example, the first mixed solution also contains one or more components selected from the following group:
[0197] 0.1-5 parts by weight of cellulose thickener;
[0198] The pH regulator of 0.01-1 weight part;
[0199] 0.01-1 part by weight of wetting agent;
[0200] 0.2-5 parts by weight of silicone defoamer; and
[0201] 0-10 parts by weight of antifreeze.
[0202] In another pref...
Embodiment 1
[0253] Example 1 Paint 1
[0254] making process
[0255] Weigh 18 parts of water in the tank by weight, add 10 parts of golden pearlescent pigments with a particle size of 10-60um (the outer layer of metal oxide is titanium dioxide and ferric oxide, and the particle size of the core mica is 7-40um) Soak for use, weigh 18 parts of water and add it to the dispersion tank, control the speed at 200-300 rpm, add in order: 0.75 parts of cellulose thickener NATROSOL 250MBR, 0.1 part of organic alcohol amine pH regulator AMP950.1 parts , 0.2 parts of wetting agent SN996, 3 parts of antifreeze PEG400, 0.3 parts of silicone defoamer SN154, 28 parts of pre-soaked pearlescent pigment slurry, 3 parts of 100-mesh glass beads, 17 parts of 150-mesh glass beads, adjust the speed to 1000 rpm, disperse for 15 minutes and then control the rotation speed at 700-800 rpm, add in sequence: 0.5 parts of preservative BIOX CM, 0.5 parts of antifungal agent BIOX M248, 25 parts of pure acrylic emulsion ...
Embodiment 2
[0265] Example 2 Paint 2
[0266] making process
[0267] Take by weight 15 parts of water and the tank, add 10 parts of golden pearlescent pigments with a particle size of 10-60um (the metal oxide outer layer is titanium dioxide and ferric oxide, and the particle size of the core mica is 7-40um ) soaked for use, weighed 16 parts of water and added to the dispersion tank, the speed was controlled at 200-300 rpm, followed by adding: 0.75 parts of cellulose thickener NATROSOL 250MBR, organic alcohol amine pH regulator AMP950.1 0.2 parts of wetting agent SN996, 3 parts of antifreeze PEG400, 0.3 parts of silicone defoamer SN154, 25 parts of pre-soaked pearlescent pigment slurry, 5 parts of 100-mesh glass beads, 20 parts of 150-mesh glass beads. Adjust to 1000 rpm, disperse for 15 minutes and then control the speed at 700-800 rpm, add in order: 0.5 parts of preservative BIOX CM, 0.5 parts of antifungal agent BIOX M248, 25 parts of pure acrylic emulsion SF-266, 0.7 parts of alcoho...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com