A processing method and four-way elastic technology, which is applied in dyeing, textile material processing, liquid/gas/steam textile material processing, etc., can solve the problems of hand feeling board and small elasticity, achieve soft hand feeling, good elasticity, and avoid shrinkage. Shrink effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0046] The dyeing and finishing processing method of described T / R spandex four-way stretch fabric, concrete steps are as follows:
[0047] (1) Distribution: 950 meters per cylinder.
[0048] (2) Pretreatment of dyeing jigger: Soda ash 5g / L, degreasing agent 5g / L, heat preservation at 95°C for 60min. The incoming cloth is smooth and the winding is dense.
[0049] (3) Water drying: temperature 150°C, paddle pressure 3.0bar, speed 40m / min, cloth fall width 165cm.
[0050] (4) Scouring in high temperature and high pressure overflow dyeing machine: Soda ash 1.5g / L, refining agent 1g / L, temperature 120°C, treatment time 30min.
[0051] (5) Pre-forming: temperature 180°C, vehicle speed 40m / min, overfeed 10%, and cloth drop width 155cm.
[0052] (6) Singeing: According to the condition of the cloth surface, the singeing method of one positive and one reverse is adopted, and the singeing speed is 26Hz.
[0053] (7) Dyeing:
[0054] Disperse dyeing process prescription is:
[005...
Embodiment 2
[0067] The dyeing and finishing processing method of described T / R spandex four-way stretch fabric, concrete steps are as follows:
[0068] (1) Each cylinder is distributed 1200 meters;
[0069] (2) Pretreatment of dyeing jigger: Soda ash 5g / L, degreasing agent 5g / L, heat preservation at 95°C for 60min. The incoming cloth is smooth and the winding is dense.
[0070] (3) Water drying: temperature 160°C, paddle pressure 3.0bar, speed 50m / min, cloth fall width 165cm.
[0071] (4) Scouring in high temperature and high pressure overflow dyeing machine: Soda ash 1.5g / L, refining agent 1g / L, temperature 120°C, treatment time 30min.
[0072] (5) Pre-forming: temperature 170°C, vehicle speed 30m / min, overfeed 10%;
[0073] (6) Singeing: Two positive and one negative singeing methods are adopted, and the singeing speed is 30Hz;
[0074] (7) Dyeing: use disperse dyes and reactive dyes to dye the fabric raw materials respectively;
[0075] Dyeing process prescription and process condit...
Embodiment 3
[0082] The dyeing and finishing processing method of described T / R spandex four-way stretch fabric, concrete steps are as follows:
[0083] (1) Each cylinder is distributed 800 meters;
[0084] (2) Pretreatment of dyeing jigger: Soda ash 5g / L, degreasing agent 5g / L, heat preservation at 95°C for 60min. The incoming cloth is smooth and the winding is dense.
[0085] (3) Water-drying: temperature 140°C, paddle pressure 3.0bar, speed 50m / min, cloth fall width 165cm;
[0086] (4) Scouring of high-temperature and high-pressure overflow dyeing machine: use soda ash and refining agent for treatment;
[0087] (5) Pre-forming: temperature 190°C, vehicle speed 50m / min, overfeed 10%;
[0088] (6) Singeing: One positive and one negative singeing method is adopted, and the singeing speed is 24Hz;
[0089] (7) Dyeing: use disperse dyes and reactive dyes to dye the fabric raw materials respectively;
[0090] Dyeing process prescription and process conditions are with embodiment 1.