A reinforced concrete, power transmission and transformation technology, which is applied in building maintenance, construction, building construction, etc., can solve the problems of transmission line safety hazards, large indirect losses, and long-term power outages in the power grid, and achieve the reinforcement of axial bearing capacity and High bending resistance, high transverse crack resistance, and high rigidity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] Remove the loose concrete on the cement poles where the cracked and exposed bars and the broken and loose concrete are exposed to expose the steel bars. Grind the four sides of the concrete where the exposed ribs are damaged into beveled edges with an angle of 30°-40°; clean up the dust or loose stones and other sundries at the bottom of the exposed ribs, such as figure 1 shown.
[0038] Mix the concrete according to the proportion of C50 strength grade, add 5% expansion agent into the concrete, fill the concrete to the damaged and exposed ribs, and its surface is basically the same as the original cement rod shape, such as figure 2 shown.
[0039] Install the prestressed steel pipe after the cement solidifies and hardens, make the prestressed steel pipe and install it to the damaged place such as image 3 As shown, the specific process is:
[0040] Consult or measure the outer diameter of the reinforced concrete pole for power transmission and transformation, selec...
Embodiment 2
[0046] On the basis of completing the operation of embodiment 1, in order to prevent the crack from continuing to expand, make such as Figure 8 The prestressed steel hoop shown, the material, thickness and assembly of the steel hoop are the same as the prestressed steel pipe, and the schematic diagram of the groove of the steel pipe fastened by the bolt fastening block is as follows Figure 9 shown.
[0047] The installation principle of the steel hoop is: install one at a distance of 500mm for parts with cracks or cracks, and install one at a distance of 1000mm for parts without cracks. Steel hoops must be installed at the ends of cracks when arranging.
[0048] The butt welds on each side of the prestressed steel hoop are spot welded at two points, and the length is not less than 15mm. The welding process of the butt weld is the same as that of the prestressed steel pipe, and the steel hoop is painted with paint as a whole after welding.