Glue hanging technology for badminton processing
A technology of badminton and craftsmanship, applied in the direction of rackets, adhesives, adhesive additives, etc., can solve the problems of limited supply of raw materials, difficulty in distinguishing duck feathers from goose feathers, high feather requirements, etc., to avoid point aggregation, good aging resistance, The effect of increasing hydrophilicity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] A gluing process for badminton processing, comprising the following steps:
[0033] (1) Carry out the test of rotating and floating the shuttlecock, observe the tilted position of the shuttlecock during the rotation of the shuttlecock, and hang a metal hook in the opposite direction of the tilted position;
[0034] (2) Start the rotation again and repeat the above operation several times until the shuttlecock reaches the balance of rotation;
[0035] (3) Remove the metal hook, weigh the weight of the metal hook each time a metal hook is removed, and dispense glue at the position of the metal hook, the weight of the glue is the same as the weight of the metal hook;
[0036] (4) Put the gummed badminton into 0.9Mpa nitrogen and let it stand for 20 minutes.
Embodiment 2
[0038] A gluing process for badminton processing, comprising the following steps:
[0039] (1) Carry out the test of rotating and floating the shuttlecock, observe the tilted position of the shuttlecock during the rotation of the shuttlecock, and hang a metal hook in the opposite direction of the tilted position;
[0040] (2) Start the rotation again and repeat the above operation several times until the shuttlecock reaches the balance of rotation;
[0041] (3) Remove the metal hook, weigh the weight of the metal hook each time a metal hook is removed, and dispense glue at the position of the metal hook, the weight of the glue is the same as the weight of the metal hook;
[0042] (4) Put the gummed badminton into 0.8Mpa nitrogen and let it stand for 20 minutes.
[0043] The glue described in step (3) is made up of the following raw materials of weight part: 80 parts of methyl acrylate modified phenolic resins, 60 parts of guar gums, 20 parts of isocyanates, 15 parts of polyvi...
Embodiment 3
[0051] A gluing process for badminton processing, comprising the following steps:
[0052](1) Carry out the test of rotating and floating the shuttlecock, observe the tilted position of the shuttlecock during the rotation of the shuttlecock, and hang a metal hook in the opposite direction of the tilted position;
[0053] (2) Start the rotation again and repeat the above operation several times until the shuttlecock reaches the balance of rotation;
[0054] (3) Remove the metal hook, weigh the weight of the metal hook each time a metal hook is removed, and dispense glue at the position of the metal hook, the weight of the glue is the same as the weight of the metal hook;
[0055] (4) Put the gummed badminton into 0.9Mpa nitrogen and let it stand for 20 minutes.
[0056] The preparation method of described phenylalanine grafted carboxymethyl cellulose is:
[0057] (1) Mix phenylalanine and benzoethanol evenly, add water 1.6 times the weight of the mixture, and adjust the pH va...