A pretreatment and wood block technology, applied in wood treatment, pretreatment equipment, wood treatment details, etc., can solve problems such as not having particularly good moisture-proof, anti-corrosion, not a whole board, damaged wood, etc., to achieve wood block Easy splicing, easy absorption and application, and the effect of reducing burrs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] A method for pretreating a bed board with wooden blocks, characterized in that: it comprises the following steps,
[0032] Step 1. Select material: select the wood block material to be processed, and then put it in a ventilated and dry place to stand;
[0033] Step 2. Rinse: soak the wood block in clean water, then spray and rinse with deionized water;
[0034] Step 3. Baking: Take out the rinsed wooden blocks, then filter the water, put them into the drying equipment and dry them at a constant temperature of 75-80°C for 40-45 minutes;
[0035] Step 4. Soaking: Put the wooden block into ethanol for soaking, then take it out, put it in a drying equipment at 75-80°C and let it stand for 1-1.5 hours;
[0036] Step 5. Soak again: After drying, let it stand in a dry and ventilated place for 3-5 hours, then soak it in the wrapping solution for 1-1.5 hours, and then apply it evenly with a brush;
[0037] Step 6. Drying: Take out the painted material, and then put it in a dry...
Embodiment 2
[0052] A method for pretreating a bed board with wooden blocks, characterized in that: it comprises the following steps,
[0053] Step 1. Select material: select the wood block material to be processed, and then put it in a ventilated and dry place to stand;
[0054] Step 2. Rinse: soak the wood block in clean water, then spray and rinse with deionized water;
[0055] Step 3. Baking: Take out the rinsed wooden blocks, then filter the water, put them into the drying equipment and dry them at a constant temperature of 75-80°C for 40-45 minutes;
[0056] Step 4. Soak again: After drying, let it stand in a dry and ventilated place for 3-5 hours, then soak it in the wrapping solution for 1-1.5 hours, and then use a brush to evenly brush;
[0057]Step 5. Drying: Take out the painted material, then put it in a drying equipment at 85-90°C and let it stand for 1-1.5 hours;
[0058] The mass ratio of the wood block and clear water in the step 2 is 1:2.5;
[0059] When soaking in the ...
Embodiment 3
[0070] A method for pretreating a bed board with wooden blocks, characterized in that: it comprises the following steps,
[0071] Step 1. Select material: select the wood block material to be processed, and then put it in a ventilated and dry place to stand;
[0072] Step 2. Rinse: soak the wood block in clean water, then spray and rinse with deionized water;
[0073] Step 3. Baking: Take out the rinsed wooden blocks, then filter the water, put them into the drying equipment and dry them at a constant temperature of 75-80°C for 40-45 minutes;
[0074] Step 4. Soaking: Put the wooden block into ethanol for soaking, then take it out, put it in a drying equipment at 75-80°C and let it stand for 1-1.5 hours;
[0075] The mass ratio of the wood block and clear water in the step 2 is 1:2.5;
[0076] The concentration of the ethanol solution is 60-65%;
[0077] The mass ratio of the wood block to the ethanol solution is 1:2.1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com