Dry grain, dry grain glaze and dry grain glazed tile
A technology of dry granule glaze and dry granule, which is applied in the field of dry granule glaze and dry granule glazed tiles, and dry granule. Warm and comfortable touch
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Follow the steps below to prepare dry grain glazed tiles:
[0036] 1. The bricks laid by the press are dried to remove the free water inside, so that the moisture content of the bricks is less than 0.5%. After the bricks leave the drying kiln, water is sprayed on the surface of the bricks to form a layer of water film on the surface;
[0037] 2. Then pour the bottom glaze on the surface of the green body, the amount of glaze is 87g (340*670 tray); the bottom glaze includes SiO by mass percentage 2 40%, Al 2 o 3 15%, CaO10%, MgO8%, ZnO15%, K 2 O6%, Na 2 O3%, BaO3%;
[0038] 3. The inkjet machine sprays the pattern and dries it in the second drying kiln to shorten the drying time of the ink;
[0039] 4. Spray dry granular glaze; the flow rate of dry granular glaze is 26s, the specific gravity is 1.27g / ml, the glaze amount is 67g (340*670 tray), and the fineness is 0.4% by weight of dry material after passing through a 200 mesh sieve; Granular glaze is calculated in ...
Embodiment 2
[0046] Follow the steps below to prepare dry grain glazed tiles:
[0047] 1. The bricks laid by the press are dried to remove the free water inside, so that the moisture content of the bricks is less than 0.5%. After the bricks leave the drying kiln, water is sprayed on the surface of the bricks to form a layer of water film on the surface;
[0048] 2. Then pour the bottom glaze on the surface of the green body, the amount of glaze is 93g (340*670 tray); the bottom glaze includes SiO by mass percentage 2 55%, Al 2 o 3 13%, CaO8%, MgO5%, ZnO10%, K 2 O5%, Na 2 O2%, BaO2%;
[0049] 3. The inkjet machine sprays the pattern and dries it in the second drying kiln to shorten the drying time of the ink;
[0050] 4. Spray dry granular glaze; the flow rate of dry granular glaze is 31s, the specific gravity is 1.23g / ml, the glaze amount is 73g (340*670 tray), and the fineness is 0.6% by weight of dry material after passing through a 200 mesh sieve; Granular glaze is calculated in p...
Embodiment 3
[0057] Follow the steps below to prepare dry grain glazed tiles:
[0058] 1. The bricks laid by the press are dried to remove the free water inside, so that the moisture content of the bricks is less than 0.5%. After the bricks leave the drying kiln, water is sprayed on the surface of the bricks to form a layer of water film on the surface;
[0059] 2. Then pour the bottom glaze on the surface of the green body, the amount of glaze is 90g (340*670 tray); the bottom glaze includes SiO by mass percentage 2 54%, Al 2 o 3 10%, CaO9%, MgO7%, ZnO14%, K 2 O4%, Na 2 O1%, BaO1%;
[0060] 3. The inkjet machine sprays the pattern and dries it in the second drying kiln to shorten the drying time of the ink;
[0061] 4. Spray dry granular glaze; the flow rate of dry granular glaze is 29s, the specific gravity is 1.25g / ml, the glaze amount is 70g (340*670 tray), and the fineness is 0.5% by weight of dry material after passing through a 200-mesh sieve; Granular glaze is calculated in p...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com