A technology of high-strength concrete and glue reducing agent, which is applied in the field of concrete admixtures, can solve the problems that the water loss of concrete cannot be reduced, and the impermeability and durability of concrete cannot be improved, so as to reduce concrete cracks, reduce viscosity, and improve impermeability. Effects of sex and durability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] A kind of high-strength concrete glue reducer of the present embodiment is made up of the raw material of following percentage by weight: diethylene glycol 5%, styrene emulsion 0.6%, sodium silicate 8%, 104PG-50 foam control agent 0.2%, surplus is water;
[0033] A kind of preparation method of adhesive reducer for high-strength concrete comprises the following steps:
[0034] a. Modification of interface enhanced compact components
[0035] Weigh the sodium silicate, styrene emulsion and water in proportion and add them into an emulsification tank at 2000-3000rpm and stir at high speed for 15-20 minutes, stop stirring to obtain the modified interface enhanced compact component.
[0036] b. Preparation of glue reducer
[0037]1. Weigh 104PG-50 foam control agent in proportion and add it to the modified interface enhanced compact component, and stir at a medium speed of 500-600rpm for 10-15 minutes.
[0038] 2. Weigh a certain amount of diethylene glycol in proportion...
Embodiment 2
[0040] A high-strength concrete glue reducer in this embodiment is composed of the following raw materials in weight percentage: 7% polyetheramine, 0.7% styrene emulsion, 8% potassium silicate, 0.3% DA740 foam control agent, and the balance is water;
[0041] A kind of preparation method of adhesive reducer for high-strength concrete comprises the following steps:
[0042] a. Modification of interface enhanced compact components
[0043] Potassium silicate, styrene emulsion, and water are weighed in proportion and added to an emulsification tank for high-speed stirring for 15 to 20 minutes, and the stirring is stopped to obtain a modified interface-reinforced compact component.
[0044] b. Preparation of glue reducer
[0045] 1. Weigh the DA740 foam control agent in proportion and add it to the modified interface-enhanced compact component, and stir at a medium speed for 10-15 minutes.
[0046] 2. Weigh a certain amount of polyetheramine according to the proportion and slowl...
Embodiment 3
[0048] A high-strength concrete glue reducer of this embodiment is composed of the following raw materials in weight ratio: 5% diethylene glycol, 0.5% butadiene monomer emulsion, 9% sodium fluorosilicate, 0.15% 104PG-50 foam control agent , the balance is water;
[0049] A kind of preparation method of adhesive reducer for high-strength concrete comprises the following steps:
[0050] a. Modification of interface enhanced compact components
[0051] Weigh sodium fluorosilicate, butadiene monomer emulsion, and water in proportion, add them into an emulsification tank and stir at high speed for 15 to 20 minutes, stop stirring to obtain a modified interface-reinforced compact component.
[0052] b. Preparation of glue reducer
[0053] 1. Weigh 104PG-50 foam control agent in proportion and add it to the modified interface-enhanced compact component, and stir at a medium speed for 10-15 minutes.
[0054] 2. Weigh a certain amount of diethylene glycol in proportion and slowly add...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com