Cement floor construction method
A construction method and cement technology, applied in the direction of floors, buildings, building structures, etc., can solve the problems of ground compressive strength, easy separation, weak cohesion, etc., to improve the compressive strength and enhance the cohesive strength , the effect of improving the compactness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0081] A cement floor construction method includes the following steps:
[0082] S1, grassroots treatment, as follows:
[0083] First, clean the dust, scum, oil, and debris on the base layer, and use cement mortar or fine stone concrete to fill in the obvious recesses on the base layer to make the surface of the base layer level.
[0084] S2, wetting the base layer, as follows:
[0085] Sprinkle water on the base layer to moisten it the day before construction, and remove the accumulated water on the base layer in time.
[0086] S3, stucco cement paste layer, as follows:
[0087] Portland cement and water are mixed in a ratio of 1:0.4 to prepare plain cement slurry, and a layer of plain cement slurry is painted on the surface of the wet base in time to form a plain cement slurry layer.
[0088] S4. Lay fine stone concrete cushion, as follows:
[0089] While painting the plain cement slurry, pour fine stone concrete on the plain cement slurry layer to form a fine stone concrete cushion, smo...
Embodiment 2
[0109] The difference from Example 1 is:
[0110] The plain cement slurry in step S3 is mixed with Portland cement and water in a ratio of 1:0.43 to prepare plain cement slurry.
[0111] The laying thickness of the fine stone concrete cushion in step S4 is 4.5 cm.
[0112] In step S5, the laying thickness of the cement bonding layer is 7.5 cm.
[0113] The distance between adjacent gray cakes in step S6 is 1.8m.
[0114] The laying thickness of the surface layer in step S7 is 32.5 cm.
[0115] The curing and molding in step S11 are as follows:
[0116] After the third time of rubbing for 11 hours, cover the surface layer with a mulch and sprinkle water 3-4 times a day to keep the surface layer moist, control the curing temperature to 25°C-30°C, and control the curing time to 29 days.
Embodiment 3
[0118] The difference from Example 1 is:
[0119] The plain cement slurry in step S3 is mixed with Portland cement and water in a ratio of 1:0.45 to prepare plain cement slurry.
[0120] The laying thickness of the fine stone concrete cushion in step S4 is 5 cm.
[0121] In step S5, the laying thickness of the cement bonding layer is 10 cm.
[0122] In step S6, the distance between adjacent gray cakes is 2m.
[0123] The laying thickness of the surface layer in step S7 is 35 cm.
[0124] The curing and molding in step S11 are as follows:
[0125] After the third time of rubbing for 12 hours, cover the surface layer with a mulch and sprinkle water 3-4 times a day to keep the surface layer moist. The curing temperature is controlled to 25°C-30°C and the curing time is 30 days.
PUM
| Property | Measurement | Unit |
|---|---|---|
| Thickness | aaaaa | aaaaa |
| Thickness | aaaaa | aaaaa |
| Thickness | aaaaa | aaaaa |
Abstract