Embodiment 1
[0038] This embodiment provides a preparation method and application of reflective anti-counterfeiting ink, which specifically includes the following steps:
[0039] S1. Weighing: Weigh the components of the reflective anti-counterfeiting ink in proportion, and the mass percentages of each component are as follows: 500 mesh glass beads 6%, water-based polyurethane 46%, pure water 7%, absolute ethanol 30%, sulfur Diisooctyl Sodium Diethylsuccinate Anionic Surfactant 5%, Defoamer 3%, Fumed Silica 3%;
[0040] S2. Prepare the solvent: mix pure water and absolute ethanol to obtain a solvent, add water-based polyurethane and mix evenly;
[0041] S3. Stir once: add glass beads to the solution prepared in step S1, then stir once, the stirring speed is 600r / min, and the stirring time is 30min;
[0042] S4. secondary stirring: add diisooctyl sodium sulfosuccinate anionic surfactant, defoamer and anti-sedimentation agent to the solution stirred in step S2, carry out secondary stirring,...
Embodiment 2
[0046] This embodiment provides a preparation method and application of reflective anti-counterfeiting ink, which specifically includes the following steps:
[0047] S1. Weighing: Weigh each component of the reflective anti-counterfeiting ink in proportion, and the mass percentage of each component is as follows: 400 mesh glass beads 10%, water-based polyurethane 50%, pure water 10%, absolute ethanol 20%, sulfur Diisooctyl sodium diethyl succinate anionic surfactant 5%, defoamer 3%, fumed silica 2%;
[0048] S2. Prepare the solvent: mix pure water and absolute ethanol to obtain a solvent, add water-based polyurethane and mix evenly;
[0049] S3. Stir once: add glass beads to the solution prepared in step S1, then stir once, the stirring speed is 600r / min, and the stirring time is 30min;
[0050] S4. secondary stirring: add diisooctyl sodium sulfosuccinate anionic surfactant, defoamer and anti-sedimentation agent to the solution stirred in step S2, carry out secondary stirring...
Embodiment 3
[0053] This embodiment provides a preparation method and application of reflective anti-counterfeiting ink, which specifically includes the following steps:
[0054] S1. Weighing: Weigh the components of the reflective anti-counterfeiting ink in proportion. The mass percentages of each component are as follows: 450 mesh glass beads 18%, water-based polyurethane 60%, pure water 6%, absolute ethanol 22%, sulfur 1% diisooctyl sodium diethyl succinate anionic surfactant, 2% defoamer, 1% fumed silica;
[0055] S2. Prepare the solvent: mix pure water and absolute ethanol to obtain a solvent, add water-based polyurethane and mix evenly;
[0056]S3. Stir once: add glass beads to the solution prepared in step S1, then stir once, the stirring speed is 500r / min, and the stirring time is 20min;
[0057] S4. secondary stirring: add diisooctyl sodium sulfosuccinate anionic surfactant, defoamer and anti-sedimentation agent to the solution stirred in step S2, carry out secondary stirring, st...
PUM
Property | Measurement | Unit |
---|---|---|
particle size (mesh) | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com