Silk brush fibre and its preparation method
A technology of silk and bristles, which is applied in the direction of bristles, brushes, textiles and papermaking, etc., can solve the problems such as the adverse effects of bristles on the human body and the environment, and achieve the effects of low product cost, easy promotion and application, and pollution reduction
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] A bristle, comprising a core fiber formed by sticking together a plurality of silks, and a covering layer made of silk protein covering the periphery of the core fiber. The specific processing steps are:
[0017] 1. Silk degumming: with a concentration of 0.05% Na 2 CO 3 The solution degummed the silk fiber three times to ensure that the sericin on the silk was completely removed.
[0018] 2. Preparation of silk protein solution: with a concentration of 0.05% Na 2 CO 3 The solution is used to completely degumming the waste silk; the molar ratio is CaCl 2 :H 2 O:C 2 h 5 OH=1:8:2 to configure the solution. Put the degummed silk into the above solution, heat to 80±5°C, and stir at this temperature until the silk is completely dissolved. The obtained silk fibroin solution is filtered, dialyzed and concentrated to obtain a silk fibroin solution with a solid content of 65%.
[0019] 3. Bonding of silk fibers: Take 7 silks that have been completely degummed, glue the...
Embodiment 2
[0023] According to the method described in step 1 in Example 1, completely degummed silk was obtained; according to the method described in step 2, a silk fibroin solution was obtained, and the solid content of the silk fibroin was controlled at 40%.
[0024] Take 20 completely degummed silks, stick them together with the above-mentioned silk protein solution, and dry them at a temperature of 50±5°C to make silk core fibers.
[0025] The silk protein solution is coated on the surface of the prepared silk core fiber by a coating method, and then dried. Repeat this step 5 times as needed.
[0026] Steam the above-mentioned silk fibers with steam at a temperature of 120±15°C for more than 30 minutes, harden and insolubilize them with high-pressure steaming, and cut off the obtained fibers according to the length requirements, so as to obtain the multi-silk sticky silk fibers according to the present invention. Combined together to form the core fiber, the periphery is silk bris...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com