A technology of auxiliaries and formulations, which is applied in the field of one-dose auxiliaries for polyester dyeing, can solve problems such as dyeing defects, inconvenient use, and poor compatibility of auxiliaries, and achieve improved dyeing quality, good use effect, and stable all-in-one Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0072] The formula of auxiliary agent consists of by weight:
[0073] Citric Acid 15%
[0074] Aminotrimethylenephosphonic acid 3%
[0075] Polyacrylic acid (molecular weight 60000~70000) 3%
[0076] NNO 15%
[0077] Polyethylene glycol 400 monooleate 6%
[0078] Nonionic polyacrylamide (molecular weight 7-8 million) 1%
[0079] Polyoxyethylene terephthalate (molecular weight 7000-8000) 2%
[0080] Water 55%.
[0081] Preparation:
[0082] Add an appropriate amount of water, and stir at 40-50°C to add all the materials in order according to weight percentage and mix for 2-3 hours, dissolve evenly, filter and discharge.
[0083] Dyeing process steps:
[0084] Add the one-dose auxiliaries and disperse dyes of this example into the dyeing bath, dye the polyester fabric at 50°C, raise the temperature to 130°C at a rate of 1°C every 2-3 minutes, keep it warm for 45-60 minutes, then slowly cool down and put foot water , and then reduced cleaning with sodium dithionite and c...
Embodiment 2
[0142] The formula of auxiliary agent consists of by weight:
[0143] Hydrolyzed polymaleic anhydride (molecular weight 400-800) 20%
[0144] Hydroxyethylenediphosphonic acid 5%
[0145] Polyacrylic acid (molecular weight 60000~70000) 7%
[0146] NNO16%
[0147] Polyethylene glycol (400) monooleate 8%
[0148] Nonionic polyacrylamide (molecular weight 7-8 million) 2%
[0149] Polyoxyethylene terephthalate (molecular weight 7000-8000) 2%
[0150] water 40%
[0151] Preparation:
[0152] Add an appropriate amount of water, and stir at 40-50°C to add all the materials in order according to weight percentage and mix for 2-3 hours, dissolve evenly, filter and discharge.
[0153] Dyeing process steps:
[0154] Add the one-dose auxiliary agent and disperse dye of the present invention into the dyeing bath, dye the polyester fabric at 50°C, raise the temperature to 130°C at a rate of 1°C every 2-3 minutes, keep it warm for 45-60 minutes, then slowly cool down and put foot wate...
Embodiment 3
[0165] The formula of auxiliary agent consists of by weight:
[0166] Hydrolyzed polymaleic anhydride (molecular weight 400-800) 20%
[0167] Hydroxyethylenediphosphonic acid 5%
[0168] Polyacrylic acid (molecular weight 60000~70000) 7%
[0169] NNO18%
[0170] Polyethylene glycol (400) monooleate 8%
[0171] Water 42%
[0172] Preparation:
[0173] Add an appropriate amount of water, and stir at 40-50°C to add all the materials in order according to weight percentage and mix for 2-3 hours, dissolve evenly, filter and discharge.
[0174] Dyeing process steps:
[0175] Add the one-dose auxiliary agent and disperse dye of the present invention into the dyeing bath, dye the polyester fabric at 50°C, raise the temperature to 130°C at a rate of 1°C every 2-3 minutes, keep it warm for 45-60 minutes, then slowly cool down and put foot water, Then reduce and wash with sodium dithionite and caustic soda at 85°C for 15 minutes, put foot water, and then wash with water.
[0176]...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 