[0028] Select 96 parts of latex polymer resin (produced by Wuxi Xishen Daily Chemical Products Factory, also known as latex (emulsion) resin), 6 parts of red pigment (also known as magenta), 3 parts of wax, and 15 parts of silicon dioxide.
[0029] Put the above-mentioned latex polymerized polymer resin, red pigment and wax together, and stir evenly to make a mixed solution;
[0030] Then use a spray dryer to spray dry the above mixed solution into granular materials at a temperature of 250°C;
[0031] After that, the above-mentioned granular materials are screened by air classification to remove particles with a particle size greater than 12 microns and less than 1 micron;
[0032] Finally, put the screened granular material into the mixer, add silicon dioxide, and mix evenly to make red toner.
no. 2 example
[0034] Select 70 parts of latex polymeric polymer resin (produced by Wuxi Xishen Daily Chemical Products Factory or Wuxi Yusheng Chemical Co., Ltd., also known as latex (emulsion) resin), 5 parts of red pigment, 2 parts of polypropylene wax, 7 parts of silica, 0.5 parts of hexamethyldisilazane and 0.5 parts of dimethyldichlorosilane. First put the latex polymer resin, red pigment and wax together, stir evenly to make a mixed solution;
[0035] Then use a spray dryer to spray dry the above mixed solution into granular materials at a temperature of 160°C;
[0036] Afterwards, the above-mentioned granular materials are classified and screened using airflow classification equipment to remove particles with a particle size greater than 12 microns and less than 1 micron;
[0037] Finally, put the screened granular material into a mixer, add silicon dioxide, hexamethyldisilazane and dimethyldichlorosilane, and mix evenly to make red toner.
no. 3 example
[0039] Select 85 parts of latex polymer resin, 10 parts of red pigment, 5 parts of wax, 11 parts of silicon dioxide, 3 parts of hexamethyldisilazane and 3 parts of dimethyldichlorosilane. Wherein: said latex polymeric polymer resin is the product of Wuxi Xishen Daily Chemical Products Factory; said wax is polyethylene wax;
[0040] First put the latex polymer resin, red pigment and wax together, stir evenly to make a mixed solution;
[0041] Then use a spray dryer to spray dry the above mixed solution into granular materials at a temperature of 300°C;
[0042] Afterwards, the above-mentioned granular materials are classified and screened using airflow classification equipment to remove particles with a particle size greater than 12 microns and less than 1 micron;
[0043] Finally, put the screened granular material into a mixer, add silicon dioxide, hexamethyldisilazane and dimethyldichlorosilane, and mix evenly to make red toner.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com