Embodiment 1
[0053] The coating formula for the color surface of carbonless copy paper for water-based inkjet printing of barcode symbols, by weight, includes the following components:
[0054] Water 840kg
[0055] Sodium polyacrylate 5kg
[0056] Activated clay 30kg
[0057] Kaolin 60kg
[0058] Calcium carbonate 102kg
[0059] SBR Latex 15kg
[0060] Styrene Acrylic Latex 15kg
[0061] Starch glue 100kg
[0062] Zinc Salicylate 13kg
[0063] Phenolic resin 13kg
[0064] Polyvinylpyrrolidone 8kg
[0065] Hexasulfonic acid-bis(triazolphenylamine) 1,2 stilbene 3kg
[0066] Fatty alcohol polyoxyethylene ether 1kg
[0067] Fatty acid sodium 1kg,
[0068] The chemical composition of activated clay described therein is: 87% SiO 2 ;10% Al 2 o 3 ; 2% Fe 2 o 3 ; 1% MgO, activated clay can offset the effect of compound glue on color development, making the color development effect better.
[0069] The particle size of the kaolin is 1000 mesh, and the particle size of the calcium carb...
Embodiment 2
[0078] The coating formula for the color surface of carbonless copy paper for water-based inkjet printing of barcode symbols, by weight, includes the following components:
[0079] Water 700kg
[0080] Sodium polyacrylate 2kg
[0081] Activated clay 15kg
[0082] Kaolin 50kg
[0084] SBR latex 14.7kg
[0085] Styrene Acrylic Latex 18.38kg
[0086] Starch glue 92.92kg
[0087] Zinc Salicylate 8kg
[0088] Phenolic resin 12kg
[0089] Polyvinylpyrrolidone 3kg
[0090] Hexasulfonic acid-bis(triazolphenylamine) 1,2 stilbene 3kg
[0091] Fatty alcohol polyoxyethylene ether 1kg
[0092] Fatty acid sodium 1kg,
[0093] The chemical composition of activated clay described therein is: 77% SiO 2 ;16% Al 2 o 3 ; 4% Fe 2 o 3 ; 6% MgO, activated clay can offset the effect of composite glue on color development, making the color development effect better.
[0094] The particle diameter of the kaolin is 1000 mesh, and the particle diameter of ...
Embodiment 3
[0104] This is embodiment 3 of the present invention, and difference with embodiment 1 is, the coating formulation of water-based ink jet printing barcode symbol with carbonless copying paper color development surface, by weight, comprises the following components:
[0105] Water 900kg
[0106] Sodium polyacrylate 10kg
[0107] Activated clay 40kg
[0108] Kaolin 70kg
[0109] Calcium carbonate 110kg
[0110] SBR latex 16.14kg
[0111] Styrene Acrylic Latex 16.14kg
[0112] Starch glue 107.72kg
[0113] Zinc Salicylate 15kg
[0114] Phenolic resin 15kg
[0115] Polyvinylpyrrolidone 3kg
[0116] Hexasulfonic acid-bis(triazolphenylamine) 1,2 stilbene 3kg
[0117] Fatty alcohol polyoxyethylene ether 2.5kg
[0118] Fatty acid sodium 2.5kg,
[0119] The chemical composition of activated clay described therein is: 80% SiO 2 ;12% Al 2 o 3 ;3% Fe 2 o 3 ; 5% MgO, activated clay can offset the effect of composite glue on color development, making the color development ef...
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com