Non-woven fabric environmental-protection water-based ink and preparation method thereof
A water-based ink, non-woven technology, applied in the direction of ink, dyeing, textiles and papermaking, etc., can solve the problems of easy cracking, wrinkling, easy discoloration, etc., and achieve the effect of high adhesion, soft texture and bright color
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0060] A kind of non-woven environment-friendly water-based printing ink, it comprises the following preparation steps: (a) add 20.3 parts of acrylic resins, 2 parts of Digao 760W dispersants, 0.2 parts of Digao 805 defoamers and 10 parts of deionized water in a container, Mix well, then add 15 parts of high-performance organic pigment phthalocyanine green (PG.7), stir evenly, and then grind to a fineness of 9 microns by a grinder to prepare a color paste.
[0061] (b) Mix the color paste prepared in step (a) with 30 parts of self-crosslinking acrylic emulsion, 20 parts of acrylic emulsion, 2 parts of Mitsubishi W410 wax paste and 0.5 part of Dow Corning DC51 organic anti-scratch agent.
[0062] (c) Measure the viscosity with Chaishi cup 4#, the viscosity is 25sec / 25℃; the color difference △T2=5; the pH value is 8.0, and the inspection is qualified, that is, the finished product.
Embodiment 2
[0064] A non-woven environment-friendly water-based ink, which comprises the following preparation steps: (a) add 18 parts of acrylic resin, 1 part of ADDITOL VXW6394 dispersant, 0.1 part of TEGO-825 defoamer and 8 parts of deionized water in a container, fully Mix, then add 6 parts of high-performance organic pigment phthalocyanine blue and 6 parts of titanium dioxide, stir evenly, and then grind to a fineness of 6 microns through a grinder to prepare a color paste.
[0065](b) Mix the color paste prepared in step (a) with 25 parts of self-crosslinking acrylic emulsion, 15 parts of acrylic emulsion, 1 part of LUMAX AF-29 wax paste and 0.5 part of TROYSOL MS-2 organic anti-scratch agent.
[0066] (c) Measure the viscosity with Chaishi cup 4#, the viscosity is 20sec / 25℃; the color difference △T2=3; the pH value is 8.5, and the inspection is qualified, that is, the finished product.
Embodiment 3
[0068] A non-woven environment-friendly water-based ink, which comprises the following preparation steps: (a) adding 25 parts of acrylic resin, 5 parts of SURFYLNOL CT-151 dispersant, 0.5 part of Lubrizol 384 defoamer and 15 parts of deionized water in a container 5 parts, fully mixed, then add 5 parts of high-performance organic pigments phthalocyanine green, 5 parts of phthalocyanine blue, 4 parts of carbon black, 4 parts of titanium dioxide, stir evenly, and then grind to a fineness of 3 microns through a grinder to obtain a color paste .
[0069] (b) Mix the color paste prepared in step (a) with 35 parts of self-crosslinking acrylic emulsion, 25 parts of acrylic emulsion, 5 parts of ACUMIST 3105B wax paste and 0.8 part of Dow Corning DC51 organic anti-scratch agent.
[0070] (c) Measure the viscosity with Chaishi cup 4#, the viscosity is 23sec / 25℃; the color difference △T2=2; the pH value is 9, and the inspection is qualified, that is, the finished product.