Embodiment 1
[0027] A kind of 18.5tex knitting yarn blended with ecological kapok fiber and colored fiber, the mass percentage content of fiber raw materials is: kapok fiber: 50%, colored fiber: 50%, wherein: colored fiber is a mixture of combed cotton fiber and cashmere.
[0028] The production technology of the knitting yarn of above-mentioned ecological kapok fiber and colored fiber blending, comprises the following steps:
[0029] (1) Pretreatment
[0030] at a temperature of 25 o Under the condition of C, humidify the kapok fiber, control the relative humidity at 75%, add an antistatic agent at the same time, the dosage is 1.0%, and put it in a stew for 24 hours, stirring once every 6 hours;
[0031] (2) Open and clean cotton
[0032] The kapok fiber is compacted to ensure that its height and tightness are consistent with the colored fiber, and the kapok fiber and colored fiber are opened, mixed, Roll evenly, while controlling the beater speed of the catching machine to 800r / min, t...
Embodiment 2
[0044] A kind of 18.5tex knitting yarn blended with ecological kapok fiber and colored fiber, the mass percentage content of fiber raw materials is: kapok fiber: 80%, colored fiber: 20%, wherein: colored fiber is a mixture of nylon and acrylic.
[0045] The production technology of the knitting yarn of above-mentioned ecological kapok fiber and colored fiber blending, comprises the following steps:
[0046] (1) Pretreatment
[0047] at a temperature of 26 o Under the condition of C, humidify the kapok fiber and the colored fiber, and control the relative humidity at 80%, add an antistatic agent at the same time, the dosage is 2.0%, and put it for 30 hours, stirring once every 6 hours;
[0048] (2) Open and clean cotton
[0049]Compact the pretreated fibers, use automatic plucking machine, multi-bin blending machine, cotton opener and single beater lapping machine to open, mix, and evenly roll the fibers, and control the batter speed of the plucking machine to 720r at the sam...
Embodiment 3
[0061] A 18.5tex knitting yarn blended with ecological kapok fiber and colored fiber, the mass percentage content of fiber raw materials is: kapok fiber: 90%, colored fiber: 10%, wherein: the colored fiber is a mixture of cashmere and polyester.
[0062] The production technology of the knitting yarn of above-mentioned ecological kapok fiber and colored fiber blending, comprises the following steps:
[0063] (1) Pretreatment
[0064] at a temperature of 28 o Under the condition of C, humidify the kapok fiber and colored fiber, control the relative humidity at 85%, add antistatic agent at the same time, the dosage is 3.0%, and put it in a stew for 36 hours, stirring once every 6 hours;
[0065] (2) Open and clean cotton
[0066] The kapok fiber and colored fiber are compacted, and the kapok fiber and colored fiber are opened, mixed, and rolled evenly by using automatic plucking machine, multi-bin blending machine, cotton opener and single hand roll machine, while controlling ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com