Boiler pipeline descaling agent and preparation method thereof
A descaling agent and pipeline technology, which is applied in the field of boiler pipeline descaling agent and its preparation, can solve the problems of acid or alkali corrosion of boiler pipelines, unusable boilers, reduced pipeline thickness, etc., and achieves the effect of quickly removing dirt
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] 100kg of boiler pipe descaling agent is composed of the following components by weight: 12kg of sulfamic acid, 3kg of hydrofluoric acid, 3kg of Lan-826, and the balance is water.
[0037] The preparation steps are as follows:
[0038] (1) Take some water, add sulfamic acid and hydrofluoric acid in sequence while stirring at room temperature, and stir evenly after adding (8min);
[0039] (2) In (1), add Lan-826 while stirring at room temperature, and then stir evenly after adding (8min);
[0040] (3) In (2), add water to meet 100% requirement, stir evenly (8min), and the finished product is obtained.
Embodiment 2
[0042] 100kg of boiler pipe descaling agent is composed of the following components by weight: 14kg of sulfamic acid, 5kg of hydrofluoric acid, 4kg of Lan-9001, and the balance is water.
[0043] The preparation steps are as follows:
[0044] (1) Take some water, add sulfamic acid and hydrofluoric acid in sequence while stirring at room temperature, and stir evenly after adding (9min);
[0045] (2) In (1), add Lan-9001 while stirring at room temperature, and then stir evenly after adding (9min);
[0046] (3) In (2), add water to meet 100% requirement, stir evenly (9min), and the finished product is obtained.
Embodiment 3
[0048] 100kg boiler pipe descaling agent is made up of the following components: sulfamic acid 15kg, hydrofluoric acid 6kg, urotropine 5kg, and the balance is water.
[0049] The preparation steps are as follows:
[0050] (1) Take some water, add sulfamic acid and hydrofluoric acid in turn while stirring at room temperature, and stir evenly after adding (10min);
[0051] (2) In (1), add urotropine while stirring at room temperature, and stir evenly after adding (10min);
[0052] (3) In (2), add water to meet 100% requirement, stir evenly (10min), and the finished product is obtained.
PUM
Property | Measurement | Unit |
---|---|---|
Corrosion rate | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com