[0017] 1. Drawing:
[0018] First, raise the temperature of the wire drawing machine to 250°C, add 50kg of polypropylene into the suction hopper, start the suction valve, melt the polypropylene, and extrude it from the 230 pores of the spinneret through the rod to become a melt filament; then It is cooled into a solid filament; it is drawn through a cooling tank, and then enters an air heating box at 150°C for a second draft and then wound onto a bobbin to obtain a 0.13mm monofilament;
[0019] 2. Warp: through the section warping machine, the monofilaments are neatly arranged on the warp bobbin according to the length required by the process, and poured on the warp beam as required.
[0020] 3. Weaving: put the finished loom on the machine through heald reed, warp and weft are woven into monofilament cloth through P7100 Sulzer projectile loom, during which, according to the process requirements, the warp is 0.13mm Monofilament, the warp density is 230 threads / inch, the weft ...
Embodiment 2
[0028] 1. Drawing:
[0029] First, raise the temperature of the wire drawing machine to 270°C, add 50kg of polypropylene into the suction hopper, start the suction valve, melt the polypropylene, and extrude it from the 230 pores of the spinneret through the rod to become a melt filament; then It is cooled into a solid filament; it is drawn through a cooling tank, then enters an air heating box at 160°C for a second draft, and then is wound onto a bobbin to obtain a 0.20mm monofilament;
[0030] 2. Warp: through the section warping machine, the monofilaments are neatly arranged on the warp bobbin according to the length required by the process, and poured on the warp beam as required.
[0031] 3. Weaving: put the finished loom on the machine through heddle reed, and weave the warp and weft yarns into monofilament cloth through the P7100 Sulzer projectile loom. Monofilament, the warp density is 210 threads / inch, the weft yarn is made of 840D polypropylene multifilament, which i...