Embodiment 1
[0032] A method for manufacturing pulp molded packaging products, comprising the following steps:
[0033] a. Pulping: mix the original wood pulp paper with water to obtain wood pulp after disintegrating, and the concentration of the wood pulp is 0.4%;
[0034] b. Slurry suction: the lower mold is immersed below the wood pulp liquid level, and the slurry is sucked under the negative pressure of -0.05MPa for 0.5 seconds. After the slurry suction operation is completed, the lower mold goes up to the pulp surface, and the pulp molding wet blank is obtained in the lower mold;
[0035] c. Dehydration: Continue to dehydrate the pulp molded wet base in the lower mold under the suction negative pressure of -0.05MPa. The dehydration time is 5 seconds, and the pulp molded wet base with a moisture content of 75% is obtained;
[0036] d. Molding: The lower mold and the upper mold are molded together, so that the lower mold and the upper mold are closely attached, and the pressure is 5MPa / ...
Embodiment 2
[0040] A method for manufacturing pulp molded packaging products, comprising the following steps:
[0041] a. Pulping: disintegrating straw pulp paper and mixing it with water to obtain straw pulp, the concentration of the straw pulp is 0.8%;
[0042] b. Slurry suction: The lower mold is immersed below the straw pulp liquid level, and the pulp is sucked under the negative pressure of -0.06MPa for 1 second. After the slurry suction operation is completed, the lower mold goes up to the pulp surface, and the pulp molded wet blank is obtained in the lower mold;
[0043] c. Dehydration: Continue to dehydrate the pulp molded wet base in the lower mold under the negative pressure suction of -0.06MPa. The dehydration time is 15 seconds, and the pulp molded wet base with a moisture content of 74% is obtained;
[0044] d. Molding: The lower mold and the upper mold are clamped so that the lower mold and the upper mold are closely attached, at 10MPa / cm 2 Under the action of high pressure...
Embodiment 3
[0048] A method for manufacturing pulp molded packaging products, comprising the following steps:
[0049] a. pulping: bagasse pulp is crushed and mixed with water to obtain pulp, and the concentration of the pulp is 1.2%;
[0050] b. Slurry suction: The lower mold is immersed below the pulp liquid level, and the slurry is sucked under the negative pressure of -0.06MPa for 1.5 seconds. After the slurry suction operation is completed, the lower mold goes up to the pulp surface, and the pulp molding wet blank is obtained in the lower mold;
[0051] c. Dehydration: Continue to dehydrate the pulp molded wet base in the lower mold under the negative pressure suction of -0.06MPa. The dehydration time is 20 seconds, and the pulp molded wet base with a moisture content of 72% is obtained;
[0052] d. Molding: The lower mold and the upper mold are clamped so that the lower mold and the upper mold are closely attached, at 15MPa / cm 2 Under the action of high pressure and -0.06 MPa negat...
PUM
Property | Measurement | Unit |
---|---|---|
Aperture | aaaaa | aaaaa |
Aperture | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com