Polymer solar cell active layer ink, high stability polymer solar cell and preparation method thereof
A solar cell and high-stability technology, applied in the field of solar cells, can solve the problems of easy deterioration of thin film morphology, poor stability of polymer solar cells, etc., and achieve the effects of simple and convenient preparation method, low cost and wide applicability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0047] The preparation method of the active layer ink of the above-mentioned polymer solar cell: dissolving the porphyrin compound, the acceptor material and the donor material in an organic solvent, and mixing uniformly to obtain the active layer ink, wherein the porphyrin compound is a metal porphyrin compound One or more of , protoporphyrin or isoporphyrin, the amount of the porphyrin compound is 0.5%-32% of the amount of the acceptor material.
[0048] In the preparation method of the ink of the present invention, the order in which the porphyrin compound, the acceptor material and the donor material are dissolved in the organic solvent is not limited, no matter how they are added, the technical effect of improving the stability of the active layer can be achieved, but in order to make the present invention The porphyrin compound in the ink fully interacts with the acceptor material, and excludes the entangling and wrapping of the fullerene molecules or porphyrin molecules ...
Embodiment 1
[0110] Preparation of polymer solar cell active layer ink:
[0111] Preparation of PC with o-dichlorobenzene as solvent 61 BM / BL1 (1:2%, n / n) mixed solution, mixed solution, PC 61 The concentration of BM is 20mg / ml; 61 P3HT solids of the same quality as BM, and then seal the solution, heat it on a hot stage at 60°C for 12h, take it out and cool it down to room temperature naturally.
Embodiment 2
[0113] Preparation of polymer solar cell active layer ink:
[0114] Preparation of PC with o-dichlorobenzene as solvent 61 BM / BL1 (1:4%, n / n) mixed solution, mixed solution, PC 61 The concentration of BM is 20mg / ml; 61 P3HT solids of the same quality as BM, and then seal the solution, heat it on a hot stage at 60°C for 12h, take it out and cool it down to room temperature naturally.
PUM
| Property | Measurement | Unit |
|---|---|---|
| concentration | aaaaa | aaaaa |
| conversion efficiency | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 