Phase change type reflective thermal insulation coating and preparation method thereof
A reflective thermal insulation coating and phase change technology, applied in reflective/signal coatings, coatings, etc., can solve the problems of excessive temperature difference on the surface of the coating, difficult to obtain the effect, and reduced thermal insulation effect, so as to reduce the temperature difference between day and night, avoid The effect of reducing thermal insulation and improving thermal insulation efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] A formulation of a phase-change reflective heat-insulating coating and the mass fraction of each component:
[0029] Raw material mass ratio
[0030] Silicone modified acrylate emulsion 45%
[0031] water 8%
[0032] MicroPCMs 5%
[0033] Titanium dioxide 8%
[0034] Thermal insulation powder 5%
[0035] Heavy calcium powder 10%
[0036] Kaolin 7%
[0037] Talc 7%
[0038] Propylene Glycol 2%
[0039] Auxiliary 3%.
[0040] According to the above formula, add silicone-modified acrylate emulsion, water, defoamer, wetting agent, dispersant and other additives in water in sequence, then slowly add MicroPCMs, stir at 1200 rpm for 15 minutes, Fully disperse; after the MicroPCMs are evenly dispersed, slowly add titanium dioxide and disperse for 20 minutes; slowly add other fillers, increase the speed to 2000 rpm and stir for 10 minutes, and finally add a thickener to adjust the paint to an appropriate viscosity, pack it out The material is a phase-change reflective ...
Embodiment 2
[0042] A formulation of a phase-change reflective heat-insulating coating and the mass fraction of each component:
[0043] Raw material mass ratio
[0044] Silicone modified acrylate emulsion 35%
[0045] water 10%
[0046] MicroPCMs 5%
[0047] Titanium dioxide 8%
[0048] Thermal insulation powder 8%
[0049] Heavy calcium powder 12%
[0050] Kaolin 8%
[0051] Talc 7%
[0052] Propylene Glycol 3%
[0053] Auxiliary 4%.
[0054] The preparation process is the same as in Example 1.
Embodiment 3
[0056] A formulation of a phase-change reflective heat-insulating coating and the mass fraction of each component:
[0057] Raw material mass ratio
[0058] Silicone modified acrylate emulsion 30%
[0059] water 12%
[0060] MicroPCMs 4%
[0061] Titanium dioxide 10%
[0062] Beads 9%
[0063] Heavy calcium powder 13%
[0064] Kaolin 8%
[0065] Talc 7%
[0066] Propylene Glycol 3%
[0067] Auxiliary 4%.
[0068] The preparation process is the same as in Example 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com