Activated carbon and ceramic integrated filter element and preparation method thereof
An activated carbon and integrated technology, which is applied in the field of ceramic filter elements, can solve the problems of activated carbon oxidation, achieve the effects of improving water purification performance, reducing production costs, and improving taste
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0039] An activated carbon ceramic integrated filter element is composed of raw materials with the following mass fractions:
[0040] Activated carbon 40%, diatomaceous earth 30%, kaolin 20%, clay 5% and loess 5%.
[0041] The preparation method comprises the following steps:
[0042] 1) stir
[0043] Mix all raw materials, add water and stir for 30 minutes, water accounts for 35% of raw material mass;
[0044] 2) Practicing mud
[0045] The slurry that step (1) is stirred is compressed through the mud refining machine, is placed in the clamp of compressor and is cut to cut with the length of 20cm, and cuts into cylindrical shape;
[0046] 3) Natural drying
[0047] Step (2) cylindrical carbon rod is carried out natural drying for 24 hours, obtains semi-finished product;
[0048] 4) cutting
[0049] After cutting the semi-finished product obtained in step (3) into a suitable size according to the filter element specifications, use compressed air to remove the foreign mat...
Embodiment 2
[0055] The raw materials and preparation method of Example 2 are the same as those of Example 1, the only difference is that the molding temperature is different, see Table 1 for details.
Embodiment 3
[0057] An activated carbon ceramic integrated filter element is composed of raw materials with the following mass fractions:
[0058] Activated carbon 30%, diatomaceous earth 30%, kaolin 30%, clay 5% and loess 5%.
[0059] The preparation method comprises the following steps:
[0060] 1) stir
[0061] Mix all raw materials, add water and stir for 30 minutes, water accounts for 35% of raw material mass;
[0062] 2) Practicing mud
[0063] The slurry that step (1) is stirred is compressed through the mud refining machine, is placed in the clamp of compressor and is cut to cut with the length of 20cm;
[0064] 3) Natural drying
[0065] Step (2) cylindrical carbon rod is carried out natural drying for 24 hours, obtains semi-finished product;
[0066] 4) cutting
[0067] After cutting the semi-finished product obtained in step (3) into a suitable size according to the filter element specifications, use compressed air to remove the foreign matter adhered to the surface of the...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle size (mesh) | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com