Method for dyeing shrinkproof wool fabrics
A technology of shrink-resistant wool and dyeing method, which is applied in the field of dyeing of shrink-resistant wool fabrics, can solve problems such as color and flower, and achieve the effects of preventing defects, good production effect, and simple process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0021] 72N / 1Z twisted anti-shrink wool single yarn jersey:
[0022] (1) Pretreatment process: inject 600L industrial soft water into the dyeing machine, then put 30kg of shrink-resistant wool single-yarn jersey into the dyeing machine, and after 5 minutes of cycle operation, add 600g of wool cleaning agent DEPICOL JT, 240g of soda ash, Add 1500g of Yuanmingfen into the dyeing bath, raise the temperature to 60°C and keep it warm for 20 minutes, drain it after cooling down, and wash it twice with water.
[0023] (2) Dyeing process: pour soft water into the dyeing machine, add 1500g of Yuanming powder, 1200g of Yuzhongbao C, and 600g of Abaiger B in turn, and circulate for 5 minutes, and inject 120g of acetic acid at a constant speed for 10 minutes (diluted with water to a concentration of 50%), circulated for 10 minutes, injected dye CLAUSOL YELLOW A-4G (Shanghai Xingkang Chemical Co., Ltd.) 675g, CLAUSOLORANGE A-RG (Shanghai Xingkang Chemical Co., Ltd.) 1.2g, LANASOL TURQ P-GR ...
Embodiment 2
[0027] 60N / 1S twisted anti-shrink wool jersey:
[0028] (1) Pre-treatment process: inject 300L of industrial soft water into the dyeing machine, then put 13.63kg of shrink-resistant wool jersey into the dyeing machine, and after 5 minutes of cycle operation, add 300g of wool detergent DEPICOL JT, 109g of soda ash, and Add 682g of Mingfen into the dyeing bath, raise the temperature to 60°C and keep it warm for 20 minutes, drain it after cooling down, and wash it twice with water.
[0029] (2) Dyeing process: pour soft water into the dyeing machine, add 682g of Yuanming powder, 600g of Yuzhongbao C, and 273g of Abaiger B in turn, cycle for 5 minutes, and inject 34g of acetic acid at a constant speed for 10 minutes (diluted with water to a concentration of 50 %), circulated for 10 minutes, injected dyes CLAUSOL YELLOW A-4G (Shanghai Xingkang Chemical Co., Ltd.) 1.36g, LANASOL TURQ P-GR (Huntsman Chemical Trading (Shanghai) Co., Ltd.) 10.22g, CLAUSOL BLUE A-3G (Shanghai Xingkang ...