A kind of preparation technology of pure wood pulp fine line absorbent paper
A preparation process and technology of absorbent paper, applied in the field of papermaking, can solve the problems of residue, easy to hang yarn, no pure wood pulp material, environmental protection, etc., and achieve the effect of maintaining integrity and increasing user comfort.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A preparation process of pure wood pulp fine grain absorbent paper, comprising the following steps: (1) mixing and pulping 50% of Beimu and 50% of rainbow fish, after pulping, it is decompressed by a decomposer and beaten by disc grinding, and the degree of beating is controlled at 23 degrees, wet weight 19g;
[0022] (2) The pulp after beating is stored in the pulping tank for pulp mixing. When mixing pulp, first add dry strength agent, the dosage is 5Kg / ton paper; then add wet strength agent, dosage 40Kg / ton paper; finally add softener , with an amount of 10Kg / ton of paper, all added at room temperature;
[0023] (3) Pump the above-mentioned prepared pulp to the flow delivery system, after dilution and screening, it is diluted to a concentration of 0.04% by the secondary flushing pump and pumped into the equal pressure pulp distributor, and then in the inclined wire paper machine Medium dehydration forming;
[0024] (4) After forming, the wet paper is pressed and dr...
Embodiment 2
[0026] A preparation process of pure wood pulp fine grain absorbent paper, comprising the following steps: (1) mixing and pulping 50% of Beimu and 50% of rainbow fish, after pulping, it is decompressed by a decomposer and beaten by disc grinding, and the degree of beating is controlled at 20 degrees, wet weight 20g;
[0027] (2) The pulp after beating is stored in the pulping tank for pulp blending. When blending pulp, first add dry strength agent with an amount of 15Kg / ton of paper; then add wet strength agent with an amount of 45Kg / ton of paper; finally add softener , with an amount of 15Kg / ton of paper, all added at room temperature;
[0028] (3) Pump the above-mentioned prepared pulp to the flow delivery system, after dilution and screening, it is diluted to a concentration of 0.04% by the secondary flushing pump and pumped into the equal pressure pulp distributor, and then in the inclined wire paper machine Medium dehydration forming;
[0029] (4) The formed wet paper i...
Embodiment 3
[0031] A preparation process of pure wood pulp fine grain absorbent paper, comprising the following steps: (1) mixing and pulping 50% of Beimu and 50% of rainbow fish, after pulping, it is decompressed by a decomposer and beaten by disc grinding, and the degree of beating is controlled at 26 degrees, wet weight 18g;
[0032] (2) The pulp after beating is stored in the pulping tank for pulp mixing. When mixing pulp, first add dry strength agent at an amount of 10Kg / ton of paper; then add wet strength agent at an amount of 50Kg / ton of paper; finally add softener , with an amount of 5Kg / ton of paper, all added at room temperature;
[0033] (3) Pump the above-mentioned prepared pulp to the flow delivery system, after dilution and screening, it is diluted to a concentration of 0.04% by the secondary flushing pump and pumped into the equal pressure pulp distributor, and then in the inclined wire paper machine Medium dehydration forming;
[0034] (4) The formed wet paper is then pr...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More