Embodiment 1
[0046] This embodiment provides a wood softener, which includes lithium chloride, N,N-dimethylacetamide and water, and the ratio of the three substances is 1:4:18.
[0047] This embodiment provides the preparation method of the above-mentioned wood softener. When making the above-mentioned wood softener, lithium chloride and water are mixed. After the lithium chloride is completely dissolved, N,N-dimethylacetamide is added and stirred evenly.
[0048] The present embodiment provides a kind of wood softening method, uses the above-mentioned wood softening agent to soften the sweet stone fruit wood, comprises the steps:
[0049] Step 1: Saw the drupe wood into wood samples of 15mm × 15mm × 15mm. It is required that the three cross-sections of the wood, the diameter and the string, are clearly visible to form a cross-section sample of the drupe wood, a radial section sample of the drupe wood and Pimento wood string section sample;
[0050] Step 2: Put the above-mentioned sample ...
Embodiment 2
[0061] This embodiment provides a wood softener, which includes lithium chloride, N,N-dimethylacetamide and water, and the ratio of the three substances is 1:4:18.
[0062] This embodiment provides the preparation method of the above-mentioned wood softener. When making the above-mentioned wood softener, lithium chloride and water are mixed. After the lithium chloride is completely dissolved, N,N-dimethylacetamide is added and stirred evenly.
[0063] The present embodiment provides a kind of wood softening method, uses the above-mentioned wood softener to soften red ironwood, comprises the steps:
[0064] Step 1: Saw the red iron wood into a wood sample of 15mm×15mm×15mm. It is required that the three cross-sections of the wood, the diameter and the string, are clearly visible to form the cross-section sample of the red iron wood and the radial cut surface of the red iron wood. Samples and wing red iron wood string section samples;
[0065] Step 2: Put the above-mentioned samp...
Embodiment 3
[0074] This embodiment provides a wood softener, which includes lithium chloride, N,N-dimethylacetamide and water, and the ratio of the three substances is 1:4:18.
[0075] This embodiment provides the preparation method of the above-mentioned wood softener. When making the above-mentioned wood softener, lithium chloride and water are mixed. After the lithium chloride is completely dissolved, N,N-dimethylacetamide is added and stirred evenly.
[0076] The present embodiment provides a kind of wood softening method, uses the above-mentioned wood softener to soften double-column hematoxylin, comprises the steps:
[0077] Step 1: Saw the double-column hematoxylin into a wood sample of 15mm×15mm×15mm. It is required that the three cross-sections of the wood, the diameter and the chord, are clearly visible to form a double-column hematoxylin cross-section sample and a double-column hematoxylin radial section. Samples and double-column hematoxylin string section samples;
[0078] S...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com