[0033] The invention provides a kind of preparation method of yak cashmere yarn, comprises the following steps:
[0034] Mix yak hair, health-preserving additives and water and then veneer to obtain health-preserving yak hair;
[0035] After mixing the health-preserving yak cashmere and water-soluble fiber, carding is carried out to obtain a raw sliver of the mixture;
[0036] Drawing the mixture raw sliver to obtain fiber cooked sliver;
[0037] Carrying out roving to the fiber cooked slivers to obtain roving;
[0038] Fine spinning the roving to obtain a single-ply yarn;
[0039] Paralleling the single yarns to obtain multiple yarns;
[0040] The multi-ply yarn is twisted to obtain yak cashmere yarn.
[0041] The preparation method of the yak cashmere yarn provided by the present invention is preferably carried out in the air, and the air ambient temperature is preferably 23-28°C, more preferably 24-27°C, most preferably 25-26°C; the air ambient humidity is preferably 55...
Embodiment 1
[0066] Raw material preparation: take 80% (weight ratio) of yak wool fiber and 20% (weight ratio) of water-soluble fiber.
[0067] Health care: mix according to the ratio to get health care aids: 1 part of crude oil, 0.4 parts of antistatic agent, 20 parts of water; the mixed health care aids are sprayed on the yak wool fiber according to the mass ratio of 1:100 and Stew the wool for 24 hours, and turn over the warehouse twice after 24 hours; the moisture regain is controlled at 22% to 25%.
[0068] Opening and mixing: the water-soluble fiber is sent to the opening machine for pre-opening, and the water-soluble fiber after pre-opening is mixed with the yak wool fiber processed in the previous step. The water-soluble fiber and yak wool fiber are sent to the wool feeding machine for further mixing, and the unevenness is controlled below 1.2%.
[0069] Carding: The cylinder speed of the carding machine is controlled at 260 rpm; the five-point distance between the cover plate and...
Embodiment 2
[0078] Raw material preparation: take 85% (weight ratio) of yak wool fiber and 15% (weight ratio) of water-soluble fiber.
[0079] Health care: mix according to the ratio to get the health care aids: 1 part of crude oil, 0.45 parts of antistatic agent, 21 parts of water; the mixed health care aids are sprayed on the yak wool fibers according to the mass ratio of 1:100 and Stew the wool for 24 hours, and turn over the warehouse twice after 24 hours; the moisture regain is controlled at 22% to 25%.
[0080] Opening and mixing: the water-soluble fiber is sent to the opening machine for pre-opening, and the water-soluble fiber after pre-opening is mixed with the yak wool fiber processed in the previous step. The water-soluble fiber and yak wool fiber are sent to the wool feeding machine for further mixing, and the unevenness is controlled below 1.2%.
[0081] Carding: The cylinder speed of the carding machine is controlled at 250 rpm; the five-point distance between the cover pla...
PUM
Property | Measurement | Unit |
---|---|---|
Fineness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com