Anti-wrinkle finishing agent and preparation and padding method
An anti-wrinkle finishing agent and finishing agent technology, which can be used in the processing of textile material equipment configuration, fiber processing, textile and paper making, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] 1) React citric acid and glyoxal at a molar ratio of 1:6 at 40°C for 6 hours to prepare glyoxal-modified citric acid;
[0030] 2) Add 60 kg of glyoxal-modified citric acid, 2.0 kg of fatty alcohol polyoxyethylene ether, 10 kg of cross-linking agent, and 30 g of catalyst sodium nitrate into the container, and replenish the liquid to the liquid level of 1000L. Finishing agent;
[0031] 3) The padding finishing liquid adopts the process of two dipping and two rolling, and the excess rolling rate is 78%;
[0032] 4) The pre-baking temperature is 100°C, and the baking time is 2 minutes;
[0033] 5) Baking The baking temperature is 160°C, the baking time is 150s, and then the fabric is finished.
Embodiment 2
[0035] 1) React citric acid and glyoxal at a molar ratio of 1:6 at 40°C for 6 hours to prepare glyoxal-modified citric acid;
[0036] 2) Add 60 kg of glyoxal-modified citric acid, 2.0 kg of fatty alcohol polyoxyethylene ether, 10 kg of cross-linking agent, and 30 kg of catalyst sodium citrate into the container, and replenish the liquid to the liquid level of 1000L. Finishing agent;
[0037] 3) The padding finishing liquid adopts the process of two dipping and two rolling, and the excess rolling rate is 78%;
[0038] 4) The pre-baking temperature is 100°C, and the baking time is 2 minutes;
[0039] 5) Baking The baking temperature is 160°C, the baking time is 150s, and then the fabric is finished.
Embodiment 3
[0041] 1) React citric acid and glyoxal at a molar ratio of 1:6 at 40°C for 6 hours to prepare glyoxal-modified citric acid;
[0042] 2) Add 60 kg of glyoxal-modified citric acid, 2.0 kg of fatty alcohol polyoxyethylene ether, 10 kg of cross-linking agent, and 30 kg of sodium hypophosphite catalyst into the container, and add liquid to 1000L liquid level, and prepare the product Finishing agent;
[0043] 3) The padding finishing liquid adopts the process of two dipping and two rolling, and the excess rolling rate is 78%;
[0044] 4) The pre-baking temperature is 100°C, and the baking time is 2 minutes;
[0045] 5) Baking The baking temperature is 160°C, the baking time is 150s, and then the fabric is finished.
PUM
| Property | Measurement | Unit |
|---|---|---|
| angle | aaaaa | aaaaa |
| whiteness | aaaaa | aaaaa |
| whiteness | aaaaa | aaaaa |