A water-resistant, decorative paper technology, used in inks, applications, household appliances, etc., can solve the problems of large color contrast of printing samples, dark appearance, and increased color difference of printing samples, so as to reduce the amount of solvent used and improve the quality. Unstable, Emission Reduction Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] The high water resistance decorative paper ink produced by using plant modified protein includes the following components in mass percentage: 44% of modified soybean resin, 50% of water, 0.5% of defoamer, 1% of pH regulator, wetting 0.5% agent, 3% slow drying agent, 0.5% fungicide, 0.5% thickener.
[0035] The preparation method of the ink for high water resistance decorative paper produced by adopting plant modified protein as described above comprises the following steps:
[0036] (1) Add 30% water and 0.5% defoamer in sequence in a high-efficiency grinder, grind and disperse at high speed for 120 minutes;
[0037] (2) Transfer the homogeneous mixture obtained in step (1) into a blender, and add 44% modified soybean resin, 20% water, 1% pH regulator, 0.5% wetting agent successively, and stir at a high speed 60 minutes;
[0038] (3) Add 3% slow-drying agent, 0.5% bactericide, and 0.5% thickener to the homogeneous mixture obtained in step (2), stir at high speed for 2...
Embodiment 2
[0040] The high water resistance decorative paper ink produced by using plant modified protein comprises the following components in mass percentage: 35% of modified soybean resin, 41% of water, 0.5% of defoamer, 3% of polymer dispersant, permanent Solid yellow 15%, pH regulator 1%, wetting agent 0.5%, slow drying agent 3%, bactericide 0.5%, thickener 0.5%.
[0041] The preparation method of the ink for high water resistance decorative paper produced by adopting plant modified protein as described above comprises the following steps:
[0042] (1) Add 25% of water, 0.5% of defoamer, 3% of polymer dispersant, and 15% of permanent yellow in the high-efficiency grinder in sequence, and grind and disperse at high speed for 120 minutes;
[0043] (2) After filtering the homogeneous mixture obtained in step (1), add it to the mixer, add 35% modified soybean resin, 16% water, 1% pH regulator, and 0.5% wetting agent successively, and stir at a high speed 60 minutes;
[0044] (3) Add 3...
Embodiment 3
[0046] The high water resistance decorative paper ink produced by using plant modified protein comprises the following components in mass percentage: 40% of modified soybean resin, 42% of water, 0.5% of defoamer, 2% of polymer dispersant, permanent Fast red 10%, pH adjuster 1%, wetting agent 0.5%, slow drying agent 3%, bactericide 0.5%, thickener 0.5%.
[0047] The preparation method of the ink for high water resistance decorative paper produced by adopting plant modified protein as described above comprises the following steps:
[0048] (1) Add 12% water, 0.5% defoamer, 2% polymer dispersant, and 10% permanent yellow in the high-efficiency grinder, and grind and disperse at high speed for 120 minutes;
[0049] (2) After filtering the homogeneous mixture obtained in step (1), add it into the blender, add 40% modified soybean resin, 30% water, 1% pH regulator, and 0.5% wetting agent successively, and stir at a high speed 60 minutes;
[0050] (3) Add 3% slow-drying agent, 0.5%...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com