Pulping method for improving pulping degree of softwood pulp
A technology of coniferous wood pulp and beating degree, which is applied in the direction of pulp beating method, non-fiber pulp addition, non-polymer organic compound addition, etc. It can solve the problems such as difficulty in improving beating degree, inability to change physical properties, and unsatisfactory improvement effect. Achieve the effects of improved beating degree, easy cutting and splitting
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A beating method for improving the beating degree of softwood pulp, comprising the following steps:
[0016] (1) Preparation of treatment solution: In parts by weight, take 4 parts of white vinegar, 1.5 parts of hydrogen peroxide, 1 part of persimmon leaf extract, 0.4 part of liquorice extract, and 100 parts of water, and mix them to obtain a treatment solution;
[0017] (2) Abrasive preparation: in parts by weight, including 15 parts of nano-carbon, 6 parts of nano-calcium carbonate, and 3 parts of nano-copper;
[0018] (3) Disintegrate the coniferous wood pulp board with a hydraulic pulper, and then soak it in a treatment solution at a temperature of 90°C for 3.5 hours to obtain a soaking material for use;
[0019] (4) Add abrasive material equivalent to 4.5% of its weight to the above-mentioned standby soaking material, and beat with a PFI refiner.
[0020] Wherein, the main components of the persimmon leaf extract are natural vitamin C, rutin, choline, and flavonoi...
Embodiment 2
[0023] A beating method for improving the beating degree of softwood pulp, comprising the following steps:
[0024] (1) Treatment solution preparation: in parts by weight, take 3 parts of white vinegar, 1.3 parts of hydrogen peroxide, 0.8 parts of persimmon leaf extract, 0.3 part of liquorice extract, and 100 parts of water, and mix them to obtain a treatment solution;
[0025] (2) Abrasive preparation: by weight, including 12 parts of nano-carbon, 7 parts of nano-calcium carbonate, and 2 parts of nano-copper;
[0026] (3) Disintegrate the coniferous wood pulp board with a hydraulic pulper, and then soak it in a treatment solution with a temperature of 85°C for 4 hours to obtain a soaking material for use;
[0027] (4) Add abrasive material equivalent to 3% of its weight to the above-mentioned standby soaking material, and beat with a PFI refiner.
[0028] Wherein, the main components of the persimmon leaf extract are natural vitamin C, rutin, choline, and flavonoid glycoside...
Embodiment 3
[0031] A beating method for improving the beating degree of softwood pulp, comprising the following steps:
[0032] (1) Treatment solution preparation: in parts by weight, take 5 parts of white vinegar, 1.7 parts of hydrogen peroxide, 1.2 parts of persimmon leaf extract, 0.5 part of liquorice extract, and 100 parts of water, and mix them to obtain a treatment solution;
[0033] (2) Abrasive preparation: in parts by weight, including 18 parts of nano-carbon, 5 parts of nano-calcium carbonate, and 4 parts of nano-copper;
[0034] (3) Disintegrate the coniferous wood pulp board with a hydraulic pulper, and then soak it in a treatment solution with a temperature of 95°C for 3 hours to obtain a soaking material for use;
[0035] (4) Add grinding material equivalent to 6% of its weight to the above-mentioned standby soaking material, and beat with a PFI refiner.
[0036] Wherein, the main components of the persimmon leaf extract are natural vitamin C, rutin, choline, and flavonoid ...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com