Microfiber PES synthetic leather and production process thereof
A production process, synthetic leather technology, applied in the field of synthetic leather
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] Microfiber PES synthetic leather production process steps:
[0035] (1) Evenly coat the bottom PU thermoplastic resin on the microfiber non-woven fabric through a coating machine, and the amount of the bottom PU thermoplastic resin is 20g / m 2 ;
[0036] (2) Apply the modified PES thermoplastic resin in the middle layer evenly on the bottom layer through a coating machine, and the amount of modified PES thermoplastic resin is 30g / m 2 ;
[0037] (3) The oven is heated up to 180°C and kept warm for 10s to obtain microfiber leather;
[0038] (4) Use release paper or release film to uniformly coat the modified PES thermoplastic resin on the coating machine, and the amount of modified PES thermoplastic resin is 20g / m 2 , and then transfer the resin to the superfiber leather surface layer by heat transfer on the transfer compound machine, and finally send it to the embossing machine to emboss the leather pattern to obtain the superfiber PES synthetic leather.
Embodiment 2
[0040] Microfiber PES synthetic leather production process steps:
[0041] (1) Apply the bottom PU thermoplastic resin evenly on the superfine fiber non-woven fabric through a coating machine, and the bottom PU thermoplastic resin consumption is 10g / m2;
[0042] (2) Apply the TPU thermoplastic resin in the middle layer evenly on the bottom layer through a coating machine, and the amount of TPU thermoplastic resin is 40g / m 2 ;
[0043] (3) The oven is heated up to 200°C and kept warm for 50s to obtain microfiber leather;
[0044] (4) Use release paper or release film to evenly coat the modified PES thermoplastic resin on the coating machine, and the amount of modified PES thermoplastic resin is 30g / m 2 , and then transfer the resin to the superfiber leather surface layer by heat transfer on the transfer compound machine, and finally send it to the embossing machine to emboss the leather pattern to obtain the superfiber PES synthetic leather.
Embodiment 3
[0046] Microfiber PES synthetic leather production process steps:
[0047] (1) Apply the bottom layer modified PES thermoplastic resin evenly on the superfine fiber non-woven fabric through a coating machine, and the amount of modified PES thermoplastic resin is 15g / m 2 ;
[0048] (2) Apply the TPU thermoplastic resin in the middle layer evenly on the bottom layer through a coating machine, and the amount of TPU thermoplastic resin is 20g / m 2 ;
[0049] (3) The oven is heated up to 200°C and kept warm for 30s to obtain microfiber leather;
[0050] (4) Use release paper or release film to evenly coat the modified PES thermoplastic resin on the coating machine, and the amount of modified PES thermoplastic resin is 30g / m 2 , and then transfer the resin to the superfiber leather surface layer by heat transfer on the transfer compound machine, and finally send it to the embossing machine to emboss the leather pattern to obtain the superfiber PES synthetic leather.
PUM
Property | Measurement | Unit |
---|---|---|
Granularity | aaaaa | aaaaa |
Melting point | aaaaa | aaaaa |
Granularity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com