Method of preparing building bricks by adopting gangue
A technology for coal gangue and construction, applied in applications, household utensils, clay products, etc., can solve the problems of strength, thermal insulation, poor thermal insulation mechanical properties, many pores, inseparable from a large number, etc., to achieve environmental protection , good thermal insulation and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A method for preparing building bricks from coal gangue, specifically comprising the steps of:
[0027] (1) Weigh the following raw materials in parts by weight: 30 parts of coal gangue, 20 parts of fly ash, 20 parts of weathered shale, 10 parts of silt, 12 parts of clay, 8 parts of cement, 13 parts of cotton fiber, 7 parts of wood fiber , 2.5 parts of defoamer, 1.5 parts of water reducer, 0.7 parts of early strength agent, 15 parts of water;
[0028] (2) Take coal gangue, fly ash, and weathered shale according to the weight parts and put them into the pulverizer to pulverize, sieve, collect the sieved particles, and the particle diameter of the sieved particles passes through a 40-60 mesh sieve for subsequent use;
[0029] (3) Mix the sieved granules in step 2 with half of the water and place it for 3 hours, then add the remaining water and stir for 3 hours to prepare the mixture A;
[0030] (4) Take silt, clay and cement according to parts by weight and put them into...
Embodiment 2
[0038] A method for preparing building bricks from coal gangue, specifically comprising the steps of:
[0039] (1) Weigh the following raw materials in parts by weight: 40 parts of coal gangue, 30 parts of fly ash, 25 parts of weathered shale, 15 parts of silt, 13 parts of clay, 10 parts of cement, 15 parts of cotton fiber, and 9 parts of wood fiber , 3 parts of defoamer, 1.7 parts of water reducing agent, 1 part of early strength agent, 25 parts of water;
[0040] (2) Take coal gangue, fly ash, and weathered shale according to the weight parts and put them into the pulverizer to pulverize, sieve, collect the sieved particles, and the particle diameter of the sieved particles passes through a 40-60 mesh sieve for subsequent use;
[0041] (3) Mix the sieved granules and half of the water in step 2 evenly and place it for 3 hours, then add the remaining water and stir evenly for 1.5 hours to prepare the mixture A;
[0042] (4) Take silt, clay and cement according to parts by we...
Embodiment 3
[0050] A method for preparing building bricks from coal gangue, specifically comprising the steps of:
[0051] (1) Weigh the following raw materials in parts by weight: 50 parts of coal gangue, 40 parts of fly ash, 30 parts of weathered shale, 20 parts of silt, 15 parts of clay, 12 parts of cement, 17 parts of cotton fiber, and 12 parts of wood fiber , 3.5 parts of defoamer, 2 parts of water reducer, 1.5 parts of early strength agent, 30 parts of water;
[0052] (2) Take coal gangue, fly ash, and weathered shale according to the weight parts and put them into the pulverizer to pulverize, sieve, collect the sieved particles, and the particle diameter of the sieved particles passes through a 40-60 mesh sieve for subsequent use;
[0053] (3) Mix the sieved granules and half of the water in step 2 evenly and place it for 2-4 hours, then add the remaining water and stir for 2 hours to prepare the mixture A;
[0054] (4) Take silt, clay and cement according to parts by weight and p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology