Steam-curing-free corrosion-resistant concrete pole and preparation method thereof
A technology for corrosion-resistant concrete and no steam curing, applied in the field of building materials, can solve the problems of high energy consumption of steam curing, adverse effects on the durability of concrete, accelerated concrete hardening, etc., so as to reduce the links of steam curing, achieve significant economic benefits, and improve The effect of corrosion resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0030] The concrete electric pole provided in this embodiment is applied in a chloride-salt environment and includes a reinforced skeleton of the electric pole, concrete filled and wrapped around the reinforced skeleton, and a waterproof coating, wherein the surface of the reinforced skeleton is covered with an evenly distributed anticorrosion layer. The pole is prepared through the following steps:
[0031] (1) Preparation of steel skeleton
[0032] First, soak the steel bar surface with 3mol / L NaOH solution for 10 minutes, then spray silane antirust agent on the surface, and the initial spraying amount is 10g / cm 2 , and finally use the anti-rust steel bars to make the skeleton structure of the pole, and put it into the mold that has been cleaned;
[0033] (2) Preparation of concrete
[0034]The concrete provided in this embodiment includes: early-strength cementitious material, fine aggregate, coarse aggregate, water reducer, non-chloride salt early-strength agent, anti-co...
Embodiment 2
[0042] The concrete electric pole provided in this embodiment is applied in a sulfate environment, and includes a reinforced skeleton of the electric pole, concrete filled and wrapped around the reinforced skeleton, and a waterproof coating, wherein the surface of the reinforced skeleton is covered with an evenly distributed anticorrosion layer. The pole is prepared through the following steps:
[0043] (1) Preparation of steel skeleton
[0044] First, soak the steel bar surface with 3mol / L NaOH solution for 5min, and then spray silane antirust agent on the surface, the initial spraying amount is 5g / cm 2 , and finally the steel bars after anti-rust treatment are made into pole skeleton structures of different diameters and lengths according to the design requirements, and put them into the cleaned mold;
[0045] (2) Preparation of concrete
[0046] The concrete provided in this embodiment includes: early-strength cementitious material, fine aggregate, coarse aggregate, water...
Embodiment 3
[0053] In this embodiment, except for using nano-silicon instead of some silica fume, other conditions and parameters are the same as in Example 1, wherein the addition of nano-silicon is 1.0% of the total early-strength gelling material quality, i.e. 4.65kg / m 3 , and the sum of the added amount of nano silicon and silica fume is 37kg / m 3 ); the curing temperature is 20°C, 30°C, 40°C, and the curing time is 24 hours;
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
sand rate | aaaaa | aaaaa |
power level | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com