A technology for sensing electrodes and glucose, applied in the direction of material electrochemical variables, material analysis through electromagnetic means, instruments, etc., can solve problems such as the inability to apply micro sensors, and achieve improved catalytic performance, high adjustability, and high electrochemical performance. Active area effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0059] A preparation method of a flexible enzyme-free glucose sensing electrode modified by a rare earth-doped cobalt-phosphorus ternary alloy modified nanoporous copper, specifically comprising the following steps:
[0060] (1) Platinum plating on the counter electrode of the standard integrated three-electrode;
[0061] (2) modifying silver-silver chloride on the reference electrode of the standard integrated three-electrode;
[0062] (3) electrodepositing a copper layer on the working electrode of the standard integrated three-electrode;
[0063] (4) electrodepositing a gold-tin alloy on the front of the working electrode, and then removing the metal tin to obtain an electrode modified with nanoporous copper;
[0064] (5) Electrodepositing a rare earth-doped cobalt-phosphorus ternary alloy compound or a cobalt-phosphorus compound on the front of the working electrode to obtain a Co-M-P / NPC modified flexible enzyme-free glucose sensing electrode.
[0065] Further, in step ...
Embodiment 1
[0074] M=blank, preparation of Co-M-P / NPC composite electrode:
[0075] (1) The counter electrode of the standard integrated three-electrode is connected separately, and the standard platinum electrode is used as the counter electrode, and it is electrodeposited at a potential of -0.4V for 15 minutes, and the platinum plating solution is composed of H 2 PtCl 6 1mM and KCl 0.1M.
[0076] (2) The reference electrode of the standard integrated three-electrode is connected separately, and the silver wire electrode is used as the counter electrode, so that the current density is 0.3A / dm at 25°C 2 Electrodeposition for 20min in the same environment, the composition of silver-plated-silver chloride solution is: silver nitrate 40g / L, sodium thiosulfate 200g / L, potassium metabisulfite 40g / L, ammonium acetate 20g / L, thiosemicarbazide 0.6g / L.
[0077] (3) Washing, degreasing and washing the standard integrated three-electrode modified counter electrode and reference electrode, then c...
Embodiment 2
[0084] Preparation of M=La, Co-M-P / NPC composite electrode:
[0085] (1) The counter electrode of the standard integrated three-electrode is connected separately, and the standard platinum electrode is used as the counter electrode, and it is electrodeposited at a potential of -0.4V for 15 minutes, and the platinum plating solution is composed of H 2 PtCl 6 1mM and KCl 0.1M.
[0086] (2) The reference electrode of the standard integrated three-electrode is connected separately, and the silver wire electrode is used as the counter electrode, so that the current density is 0.3A / dm at 25°C 2 Electrodeposition for 20min in the same environment, the composition of silver-plated-silver chloride solution is: silver nitrate 40g / L, sodium thiosulfate 200g / L, potassium metabisulfite 40g / L, ammonium acetate 20g / L, thiosemicarbazide 0.6g / L.
[0087] (3) Washing, degreasing and washing the standard integrated three-electrode modified counter electrode and reference electrode, then conn...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com