[0065] The preparation of embodiment 1 sustained-release fragrance nanomaterial
[0066] Preparation of slow-release fragrance nanomaterials by colloid mill spray drying method:
[0067] Preparation scheme: First, take an appropriate amount of gum arabic and dissolve it in distilled water at 50-60°C. After 30 minutes, add maltodextrin into the aqueous solution of gum arabic. After dissolving, keep the temperature for 20 minutes. ℃ homogenization for 30 minutes, spray drying to obtain slow-release plant fragrance nanomaterials. Wherein, the weight ratio between gum arabic and maltodextrin is 1:1. The added amount of emulsifier is 0.3% of the mass of the whole solution. The molecular formula of the molecularly distilled monoglyceride is C 21 h 42 o 4 , the molecular weight is 358.87, and the CAS is 123-94-4.
[0068] The colloid milling method is used to prepare slow-release aromatic nanometer materials, and the spray drying method is used to prepare clathrates, which can ...
Embodiment 2~28
[0076] Example 2-28 Preparation of slow-release plant fragrance functional coating
[0077] According to the formulations in the following tables 3-1, 3-2, 3-3, prepare the slow release type plant fragrance functional coating.
[0078] The preparation method comprises the following steps:
[0079] (1) Fully stir the deionized water, dispersant, wetting agent, antifreeze, 1 / 2 defoamer, and 1 / 4 thickener in the raw material components.
[0080] (2) Under continuous stirring conditions, add titanium dioxide, 1 / 2 thickener, filler and the slow-release aromatic nanomaterial obtained in Example 1 to the material obtained in step (1), disperse at a high speed, and then transfer it to the grinder Grinding, when the product particle fineness reaches 18-22um, stop grinding.
[0081] (3) Add antifungal agent, bactericide, multifunctional additive, film-forming additive, 1 / 2 defoamer, leveling agent, 1 / 4 thickener, water-resistant environmental protection adhesive to the material obtain...