Wood core lengthening process

A technology of wood core and craftsmanship, which is applied in the direction of wood processing equipment, the joining of wooden veneers, manufacturing tools, etc., can solve the problems of large waste of raw materials, difficult processing, warping and deformation, etc., and achieve simplified production process and size Good stability and deformation correction effect

Active Publication Date: 2020-05-05
江西兴创木业有限责任公司
View PDF7 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

This method improves the utilization rate and use value of small-diameter wood, but for wood cores with a diameter of less than 6cm or even less than 3.5cm, it is very difficult to process them with the same method because they are prone to warping, deformation and cracking; and the method The steps are relatively complicated, requiring a single rough regular hexagonal prism to be finger-jointed and tenon-jointed, milled into a refined regular hexagonal prism, and then assembled to form a glued wood square, which is time-consuming and labor-intensive, which wastes a lot of raw materials, and the utilization rate of raw materials needs to be improved.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Wood core lengthening process
  • Wood core lengthening process
  • Wood core lengthening process

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0060] A wood core extension process, comprising the following steps:

[0061] S1. Timber production: The selected material is a wood core with a diameter of 2.3±0.05cm, a length of 132±0.05cm, and a moisture content of about 8.5%, and then cut to make the first hexagonal prism wood core 1 and the four-prism border wood core 2, pentagonal prism Surrounding the wood core 3, part of the first hexagonal prism wood core 1 is cut along the normal direction of the length direction to make the second hexagonal prism wood core 5 and the third 1 / 4, 3 / 4, 1 / 2 length. Hexagonal prism wood core 6, fourth hexagonal prism wood core 7, such as figure 1 , figure 2 shown;

[0062] S2. Glue application: for the first six-prism wooden core 1, four-prism border wooden core 2, five-prism border wooden core 3, second six-prism wooden core 5, third six-prism wooden core 6, fourth six-prism wooden core Wooden core 7 is coated with adhesive on the surface, and the amount of glue applied is 120g / m ...

Embodiment 2

[0072] A wood core extension process, comprising the following steps:

[0073] S1. Timber production: The selected material is a wood core with a diameter of 2.8±0.05cm, a length of 97±0.05cm, and a moisture content of about 15%, and then cut to make the first hexagonal prism wood core 1 and the four-prism border wood core 2, pentagonal prism Surrounding wood core 3, part of the first hexagonal prism wood core 1 is cut along the normal direction of the length direction to make the second hexagonal prism wood core of its 1 / 5, 4 / 5, 2 / 5, 3 / 5 length 5. The third six-prism wood core 6, the fourth six-prism wood core 7, the fifth six-prism wood core 8, such as figure 1 , image 3 shown;

[0074] S2. Glue application: for the first six-prism wooden core 1, four-prism border wooden core 2, five-prism border wooden core 3, second six-prism wooden core 5, third six-prism wooden core 6, fourth six-prism wooden core Wooden core 7 and fifth hexagonal wooden core 8 are coated with adhesi...

Embodiment 3

[0084] A wood core extension process, comprising the following steps:

[0085] S1. Timber production: The selected material is a wood core with a diameter of 3.2±0.05cm, a length of 115±0.05cm, and a moisture content of about 20%, and then cut to make the first hexagonal prism wood core 1 and the four-prism border wood core 2, pentagonal prism Surrounding wood core 3, part of the first hexagonal prism wood core 1 is cut along the normal direction of the length direction to make the second length of 1 / 6, 5 / 6, 1 / 3, 2 / 3 and 1 / 2 Hexagonal wood core 5, third hexagonal wood core 6, fourth hexagonal wood core 7, fifth hexagonal wood core 8, sixth hexagonal wood core 9, such as figure 1 , Figure 4 shown;

[0086] S2. Glue application: for the first hexagonal wood core 1, the second hexagonal wood core 5, the third hexagonal wood core 6, the fourth hexagonal wood core 7, the fifth hexagonal wood core 8, and the sixth hexagonal wood core Wooden core 9, wood core 2 surrounded by four...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
diameteraaaaaaaaaa
lengthaaaaaaaaaa
diameteraaaaaaaaaa
Login to View More

Abstract

The invention provides a wood core lengthening process. The wood core lengthening process comprises the following steps that material manufacturing is performed, wherein wood core materials are selected, and then are cut to be made into first hexagonal prism wood cores, quadrangular surrounding edge wood cores and pentagonal prism surrounding edge wood cores, and a part of the first hexagonal prism wood cores each are sectioned into two sections with different lengths in the normal direction of the length direction; gluing is performed; shaping and curing are performed; and mold stripping andmaintenance are performed. According to the wood core lengthening process, a staggered stacking method is adopted, the binding force among the wood cores is improved, assembling and lengthening are combined into one, and comb tenoning is not needed; the wood cores with the relatively large bending degrees in the length direction can also be directly used for lengthening without correction or cutting off; and the problem that the small-diameter wood cores are difficult to utilize is solved, the production process is simplified, and the obtained laminated wood is high in strength and good in quality.

Description

technical field [0001] The invention relates to the technical field of wood processing, in particular to a wood core extension process. Background technique [0002] The main raw material for the production of wood-core glulam is the residue from the production of eucalyptus veneer—the wood core after peeling the veneer. Eucalyptus is the main plantation tree species in southern my country, especially in Guangdong and Guangxi provinces, with an annual mining volume of about 50 million cubic meters. Eucalyptus is currently mainly used for peeling veneer, which is used as raw material for the production of plywood and thin wood. Each cubic meter of eucalyptus will produce about 0.07-0.1 cubic meters of core residue after rotary cutting, and the number of eucalyptus cores is about 4 million cubic meters per year. The raw materials mainly come from Shaoguan, Heyuan, Heping and Pingping areas at the junction of the west and north of Guangdong and Jiangxi, as well as Jiangxi and...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information