Unlock instant, AI-driven research and patent intelligence for your innovation.

Water-in-water coating capable of being externally toned and application of water-in-water coating

A technology of water-in-water and paint, applied in the direction of coating, etc., can solve the problems of inability to add color paste to finished products, low production efficiency, troublesome production, etc.

Active Publication Date: 2021-11-05
广东嘉宝莉科技材料有限公司
View PDF3 Cites 3 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] Although the water-in-water multi-color paint has many excellent properties, its production is very troublesome, mainly because the water-insoluble flexible film on the surface of the color particles is difficult to control, so it can only be mixed with the base paint, and the color of the color point is adjusted in advance. , it is impossible to add additional color paste to the finished product (external coloring), when the finished product is completed, there is no way to make any changes, so it is necessary to arrange a large number of coloring personnel to carefully operate, and the inventory pressure is high, and products of different colors need to be separated Packaging, batch colors, and color dot ratios vary greatly. Except for a few mainstream color numbers, they must be produced on-demand. The production efficiency is low and the production time span is long, which is not suitable for market requirements.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Water-in-water coating capable of being externally toned and application of water-in-water coating
  • Water-in-water coating capable of being externally toned and application of water-in-water coating
  • Water-in-water coating capable of being externally toned and application of water-in-water coating

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0067] The preparation method of the water-in-water coating comprises the steps of mixing the base paint and the granulation solution in a ratio greater than 2:1 by mass to prepare colored particles with a particle size of less than 1 mm, and mixing the colored particles and the continuous phase in a mass ratio of less than 1 mm. (0.25-1.5): 1 mixing step. Through such a preparation method and ratio, the content concentration of the protective glue other than the color particles in the water-in-water coating can be controlled to be less than 1%.

[0068] In one of the embodiments, at 25° C., the viscosity of the aqueous solution of hydroxyethyl cellulose containing the hydroxyethyl cellulose and the mass concentration of the hydroxyethyl cellulose is 1% is 5000 centipoise-15000 centimeters berth. Preferably, the hydroxyethyl cellulose is Ashland HE-10K.

[0069] In one embodiment, the viscosity of the first emulsion at 25° C. is 100 mP·s-3000 mP·s, and the solid content is 4...

Embodiment 1

[0119] This embodiment provides a water-in-water coating and a preparation method thereof.

[0120] (1) Preparation raw materials of water-in-water coating:

[0121] ①The base paint is prepared from the following raw materials by mass percentage:

[0122]

[0123]

[0124] ②The granulation liquid is prepared from the following raw materials by mass percentage:

[0125] Water 91.6%,

[0126] Protective glue 8% and

[0127] Second preservative 0.4%.

[0128] ③The continuous phase is prepared from the following raw materials by mass percentage:

[0129]

[0130]

[0131] (2) Preparation of water-in-water paint that can be externally tinted:

[0132] ①Prepare base paint:

[0133] Add water and hydroxyethyl cellulose into the dispersing tank, and disperse at low speed for 5 minutes; then add dispersant, wetting agent, the first defoaming agent, the first film-forming aid and the first multi-functional aid, and disperse at medium speed for 5 minutes ; Then add tit...

Embodiment 2

[0144] This embodiment provides a water-in-water coating and a preparation method thereof. Compared with Example 1, the difference is that the addition amount of water in the base paint is 77.66%, and the addition amount of the first alkali swelling thickener is 1.2%.

[0145] After testing, the strength of the water-in-water coating is good, and after adding the diluted color paste (4 parts of water, 1 part of color paste) to the finished water-in-water coating, the color particles can be tinted to achieve an external tone by adding the color paste. The effect of the finished water-in-color paint, and it can be used normally. However, the strength of the pips is slightly lower than that of Example 1.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
Login to View More

Abstract

The invention relates to water-in-water coating capable of being externally toned and application of the water-in-water coating. The coating comprises basic paint, granulation liquid and a continuous phase; the basic paint comprises 56%-80% of water, 0.5%-1.2% of hydroxyethyl cellulose, 8%-20% of acrylate emulsion, 0.4%-20% of pigment filler, 0.24%-1.12% of magnesium lithium silicate-containing protective glue and 1.2%-8% of a first alkali swelling thickener; the granulation liquid comprises 90%-95% of water and 4.8%-10% of protective glue containing magnesium lithium silicate; and the continuous phase comprises 39.2%-69.2% of water, 30%-60% of an acrylate emulsion and 0.3%-0.8% of a second alkali swelling thickener. The preparation method of the coating comprises the following steps of: mixing the base paint and the granulation liquid according to a mass ratio of more than 2: 1 to prepare the colored particles with the particle size of less than 1mm; and mixing the colored particles and the continuous phase according to a mass ratio of (0.25-1.5): 1. The coating is proper in strength and can be externally toned.

Description

technical field [0001] The invention relates to the field of coatings, in particular to a water-in-water coating capable of external coloring and application thereof. Background technique [0002] Water-in-water colorful paint, also known as liquid stone, is an all-water-based, one-time sprayed colorful granite paint, which produces vivid, durable and highly simulated colors. Compared with traditional real stone paint products, water-in-water colorful paint has the characteristics of low cost of ownership, low paint consumption during construction, easy transportation, and high raw material requirements. [0003] Although the water-in-water colorful paint has many excellent properties, its production is very troublesome. This is mainly because the water-insoluble flexible film on the surface of the color particles is difficult to control, so it can only color the basic paint and adjust the color of the color point in advance. , it is impossible to add additional color paste...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09D133/04C09D7/65C09D7/61C09D7/80C09D7/20
CPCC09D133/04C09D7/65C09D7/61C09D7/80C09D7/20C08K2003/2241C08L2205/025C08L33/04C08L1/284C08K3/34C08K3/22C08K3/346
Inventor 何兆强胡恒志
Owner 广东嘉宝莉科技材料有限公司